1 Introduction

A lithium battery bursting into flames is probably the first image one has in mind when thinking of battery safety1,2. Such thermal runaway is not limited to Li-ion cells, but can of course take place in other chemistries, such as Ni-Cd or lead acid batteries, too3. While fire and explosion are the most obvious consequences, invisible toxic gases such as CO, NO, HF, SO2 and HCl for Li-ion cells, or HS, arsine and stibine for lead acid batteries, might also be released3.

High-temperature batteries, which operate above 100 °C by definition4, are only partly susceptible to thermal runaway. A failure in the solid electrolyte of ZEBRA5,6 or Na-S cells7 will lead to short-circuit and mixing of the anodei and cathode compartments. Luckily, this is safe for ZEBRA batteries, as the reaction of Na (anode) with the catholyte (NaAlCl4) leads to the formation of solid aluminium, cell freezing and a low-impedance permanent short-circuit8–13. However, shorting a Na-S cell will lead to the formation of strongly corrosive sodium polysulphides and fast temperature increase, which can easily destroy the cell housing or seal. Much work in the past has therefore been invested to design Na-S cells inherently safe to prevent propagation of one cell’s failure to others14,15.

While safety analysis has been performed for all battery chemistries mentioned above, to our best knowledge no risk assessment has been published for Liquid Metal Batteries (LMBs)16. Such cells employ a molten salt electrolyte, which has motivated much fluid dynamic research with the idea in mind that strong flow could easily short-circuit thin electrolyte layers17,18. Short-circuits have repeatedly been observed in LMB experiments19–25 leading even to salt evaporation20. It is therefore the aim of this work to perform a thorough risk assessment of a liquid metal battery using the example of a Na-Zn cell operating at 600 °C26–28.

With regards to risk assessments, safety standards are very important as they provide guidance to identify and avoid possible risks. Of course, they depend on the country and many different standards exist. In our opinion the following are most relevant for designing safe batteries (see also Table 13):

While the standards UL 9540, IEC 62984-2 and UL 1973 must be met by any high-temperature stationary energy storage systems, the UL 9540A thermal runaway certification is harder to achieve. ZEBRA batteries sold by FZSoNick and Na-S cells from NGK comply with the latter, while Li-ion batteries usually do not33. This additional certification is the reason that ZEBRA batteries are especially popular in applications for which fire safety is critical.

2 Methods

This risk assessment follows the method defined by ISO 12100 and ISO/TR 14121-234,35. Where applicable, the following standards and regulations are considered:

As illustrated in Figure 1, the risk assessment starts with a hazard identification. Using a bottom-up approach, i.e. considering all possible ways that something can go wrong, and following the systematic methodology suggested in ISO 1210034, possible hazards are identified and listed in an Excel spreadsheet.

b2580137-ff01-476a-bbbc-81dffecace91_figure1.gif

Figure 1. Steps of the risk assessment.

The associated risk is estimated using a numerical approach by evaluating the severity score (SS), which describes the severity and extent of harm, and the probability score (PS) which accounts for the duration and frequency of harm, the probability of an event occurring and the possibility of avoiding it35. The sum of both gives the risk score (RS) – for the definitions, see Table 1.

Table 1. Definitions for risk estimation, following ISO/TR 14121-235.

severity score (SS)probability score (PS)risk score (RS = SS + PS)
%definition%definition%definition
SS ≤ 29minorPS ≤ 29remoteRS ≤ 89negligible
30 ≤ SS ≤ 89moderate30 ≤ PS ≤ 69unlikely90 ≤ RS ≤ 119low
90 ≤ SS ≤ 99serious70 ≤ PS ≤ 99likely120 ≤ RS ≤ 159medium
SS = 100catastrophicPS = 100very likelyRS ≥ 160high

After evaluating each individual risk, suitable risk reduction methods are identified34,35. Generally, inherently safe designs are always preferred. Only if this is not possible, safeguarding measures are suggested, or if unfeasible, information for safe use is provided. The Excel table containing the overview of the risk assessment can be found in Section 6.2; the details are discussed in the following.

3 Scope of the study

The life of a battery involves many phases, starting from mining of the raw materials and ending with recycling – as illustrated in Figure 2. Considering that – with the exception of AMBRIii – LMBs are not commercially available, but were mostly investigated in the laboratory, we limit the risk assessment to the use phase of experimental batteries. The cells are typically assembled in a glovebox and operated in a simple laboratory furnace.

b2580137-ff01-476a-bbbc-81dffecace91_figure2.gif

Figure 2. Phases of life of a battery.

3.1 Battery design and operation

Figure 3 shows the cell assembly, Table 2 describes the single parts28 and Section 6 provides all details of the cell design. The housing is made of welded standard components, and is closed using a CF40 vacuum flange with Cu sealing. A tube in the lid allows connecting a pressure sensor and introducing thermocouples into the cell. Current is supplied via two feedthroughs, which are connected via barrel connectors to the Mo (or W) current collectors. The active material is contained in an alumina crucible, with a ceramic sheath insulating anode and cathode. The molten salt consists usually of CaCl2-NaCl, but BaCl2, KCl, LiCl and SrCl2 might be added, too, in order to improve the electrolyte’s properties. In order to reduce self-discharge, it is split into an upper and lower compartment using a porous diaphragm, which is hold in place by a thin alumina cylinder. The cell is filled in discharged state with Zn metal and CaCl2-NaCl, which reacts according to the equation

2Na+ZnCl2↔2NaCl+Zn(1)

to Na metal and ZnCl2 at charge.

b2580137-ff01-476a-bbbc-81dffecace91_figure3.gif

Figure 3. Cell design and main dimensions28.

Table 2. Parts of the ALB and their properties28.

Densities are given for room temperature, and heat capacities for 600 °C.

partquantityspecificationdensitymasscpcomment
g/cm3gJ/(kg K)
housing11.4306 (X2CrNi19-11)7.93932060039values for 1.4301
lid11.4306 (X2CrNi19-11)7.93933560039values for 1.4301
screws61.49807.939760039values for 1.4301
tube11.4306 (X2CrNi19-11)7.9391960039values for 1.4301
bottom plate11.4306 (X2CrNi19-11)7.93910760039values for 1.4301
sealing ring1Cu9.0401143841 
diaphragm1alumina foam3.8421120043porosity 0.944
crucible1Al2O3 > 99.5 %3.84259120043 
sleeve1Al2O3 > 99.5 %3.84228120043 
diaphragm support1Al2O3 > 99.5 %3.8422120043 
barrel connector2Mo10.240229041 
screws barrel connector4A4 (1.4401)7.9390.160039values for 1.4301
anode current collector1Mo10.2401229041 
cathode current collector1Mo10.240529041 
ZnZn6.4452548146 
salt (CaCl2:NaCl)44:56 mol%
60:40 wt%
1.9473286441weighted by mass
σ = 1.38 S/cm47
feedthrough (2 pieces) 
ceramic ring1alumina3.8422120043 
lower collar1Invar 42, 1.39178.148168941cp weighted by mass
upper collar1Invar 42, 1.39178.148168941cp weighted by mass
wire1Invar 42, 1.39178.148168941cp weighted by mass
braze 11Ni-0.153541 
braze 21Au-0.414141 
sum/mean1013653cp weighted by mass

3.2 Operational limits

The cell needs to be operated within certain limits, which are summarised in Table 3 and are explained in the following.

Table 3. Operation parameters and limits of a Na-Zn LMB based on the Zn and salt amounts given in Table 2.

The values are mostly estimates, based on the experience of the authors.

propertyunittypical
value
minmaxcomment
Temperature°C600550600
OCVV1.6-1.71.21.8depends on exact salt
Current densitymA/cm21000350
Cell currentA0.2501
Overall efficiency%756090estimated
Depth of discharge%45until salt solidifies
CapacityAh0.5depends on catholyte volume
Discharge rateC/2C/161C
Energy contentWh0.9
  • Temperature: the minimum temperature is defined by solidification of the salt; the maximum temperature by the stability of the feedthroughs.

  • Open-circuit potential (OCV): Discharged cells in experiments typically exhibit 1.2 V, while the maximum predicted cell potential is 1.8 V when using the standard potentials from Hamer et al.36 and Temkin’s model for the ZnCl2 concentration in the molten salt37,38. Experimentally observed OCVs are typically in the range 1.6–1.7 V.

  • Depth of discharge (DoD): the depth of discharge can be calculated from the phase diagram, shown in Figure 4. The enrichment in CaCl2 upon charging arises because two moles of NaCl are required to produce one mole of ZnCl2. Assuming that all of the NaCl in the discharged cell (salt composition 44:56 mol% CaCl2-NaCl) reacts to form ZnCl2, a composition of 61:39 mol% CaCl2-ZnCl2 would result (0.5 * 56/(0.5 * 56 + 44) mol% ZnCl2). At an operating temperature of 600 °C, the solidus line is encountered at a salt composition of 50:35:15 mol% CaCl2-NaCl-ZnCl2. As two moles of NaCl react to one mole of ZnCl2 during discharge, the total amount of substance does not stay constant, when following the discharge line in the phase diagram. Assuming that the cell is filled with 100 mol salt, 44 mol thereof being CaCl2, 44/50 = 88 mol of salt will remain upon solidification. This results in 0.35 · 88 = 31 mol NaCl left, or 31/56 = 55 mol% left and therefore in a DoD of 45 %.

  • Operation potential window: at potentials above 2.5 V the cathode current collector could corrode, and at potentials below -0.6 V the anode current collector, see Table 16.

  • Energy density: the charge released when producing one mole of Zn is Q = 2F = 53.6 Ah because two electrons are involved in the reaction. The cell voltage is assumed to be 1.8 V as this is the maximum possible value. The mass necessary to produce one mole of Zn is given by molar masses of Na and ZnCl2 as m = 2·23 g + 136.3 g = 182.3 g. The theoretical energy density is then w = Q · U/m = 529 Wh/kg.

  • Capacity: capacity is computed such that all NaCl is consumed until solidification (see DoD) and that only the volume below the diaphragm and within the diaphragm support is taken – see Figure 3. This gives 2.65 cm3.

  • Current density: the typical current density is calculated such that it allows for operating at a voltage efficiency of 75 % – for the salt conductivity, see Table 2. The Zn surface area is used to compute the current density.

  • Operators: the cell is only operated by trained and skilled persons.

  • Mode of operation: the operation can be divided into heat-up, open circuit, charge, discharge and cool-down, further maintenance (putting cell in furnace, taking it out, connecting it), malfunctions (short-circuit, failure of housing, potentiostat failure, heating system failure) and misuse (short-circuit, overcharge, ...).

  • Environment: the cell will be operated indoors at normal air humidity, without exposure to water. The temperature of the surrounding laboratory environment will remain between 0 and 40 °C.

b2580137-ff01-476a-bbbc-81dffecace91_figure4.gif

Figure 4. Phase diagram of CaCl2-NaCl-ZnCl2 and discharge line49.

The concentration at point A (discharged) is 44:56 mol% CaCl2:NaCl, at point B (solidification) 50:35:15 mol% CaCl2:NaCl:ZnCl2 and at C (fully charged) 61:39 CaCl2:ZnCl2. The shaded area shows the compositions where the electrolyte is liquid below 600 °C.

4 Results

4.1 Intrinsic material hazards

Na-Zn LMBs employ molten metals, various salts and ceramics which may, together with their corrosion products, present certain intrinsic material hazards. Table 4 gives an overview.

Table 4. Hazards of materials and corrosion products.

The numbers in the table specify the GHS hazard category61 and are taken from GESTIS50 and various material data sheets.

irritatingcorrosivesensitisationirritatingdamagerespiratory sensitisationskin contactswallowedinhaleddamage to organsgerm cell mutagenicitycarcinogenreproductive toxicitycorrosive to metalsflammable solidreacts with watertoxic to aquatic life (acute)toxic to aquatic life (chronic)
skineyetoxicCMR
Na1B1
Zn
Ba1B1311
Ca2
K1B11
Li1B11
Sr21
BaCl2234
CaCl22
KCl
LiCl224(1A)
NaCl
SrCl21
ZnCl21B411
Na2O1B
NaOH1A11
ZnO11
Zn(OH)212
AgCl111
AuCl31B1
Cl2222311
CrCl22243
CrCl31412
CuCl214411
CuCl22144111
FeCl21B141
FeCl321141
HCl1A13
MoCl3223
MoCl51B
NiCl221133121A1B11
WCl61B14
PH31B111
fibres1B

4.1.1 Metals. While Zn metal is generally safe (although Zn vapour should not be inhaled), Na presents several risks. Cold metallic Na is corrosive to human tissue, and causes severe burns to the eyes, skin, lungs and the respiratory system50–52. Splashes in the eye are especially dangerous and can cause blindness51. Na droplets might burn even at 125 °C; thus a fire risk exists as soon as Na is in contact with air53,54. The speed at which a Na fire spreads depends crucially on its surface area, with the flames producing Na2O and Na2O2 of which 40 % end up as aerosols53. These oxides react gradually to form NaOH with air humidity and finally to Na2CO3 with carbon dioxide53. Na reacts directly with moisture, producing NaOH and hydrogen53. The latter may ignite spontaneously55, especially above 560 °C53. Air-hydrogen mixtures are flammable or explosive between 4 and 77 vol%3,50,56,57; however, with the necessary safety factors, often 1 or 2 vol% are mentioned as lower limits. Na fires can be extinguished by dry sand, cement or special metal-fire extinguishers; water and CO2 are very dangerous and must be avoided58.

Depending on the salt composition, other alkali or alkaline earth metals such as Ba, Ca, Li, K or Sr may be codeposited at the anode during charging. These should be treated in the same way as Na, as all of them may react to form appreciably corrosive oxides/hydroxides and hydrogen50. Special care is required when handling K as it reacts with air to form highly explosive peroxides50. The yellow crust on its surface can be detonated simply by cutting it with a knife59. Finally, Ba is highly toxic and its reaction products can even be absorbed through the skin50. Ba ions act as muscle stimulants and can cause death due to ventricular fibrillation59.

4.1.2 Molten salts. The hazard presented by the electrolyte depends strongly on its chemical composition:

  • BaCl2 is highly toxic and damages muscles, intestine and heart51. Its main exposure route is via the lungs50.

  • CaCl2 causes irritation of the skin and eyes, but is otherwise relatively safe50.

  • KCl is not considered a hazardous substance50.

  • LiCl is irritating for skin and eyes and toxic if swallowed50. Its reproductive toxicity is currently under discussion, with the classification cat. 1A proposed60.

  • NaCl is not considered a hazardous substance50.

  • SrCl2 is classified as eye damaging but otherwise comparably safe.

  • ZnCl2 causes strong irritation of the eyes, skin, and respiratory system, with aqueous solutions being corrosive. Exposure is possible via the skin or when swallowed, leading to damage to the intestine, kidneys and heart. ZnCl2 produces HCl when heated in air and is very toxic to aquatic life with long-lasting effects50,51.

4.1.3 Corrosion products. It is difficult to predict which exact corrosion products may appear. However, based on the components of the housing, the following should be considered:

  • active metals: NaOH, Na2O, Zn(OH)2 and ZnO might result from humidity

  • feedthrough: Au or Ag might dissolve in small amounts from the feedthrough braze

  • HCl and Cl2 gas may evolve due to hydrolysis or salt decomposition

  • sealing: Cu ions might be present

  • current collector: Mo or W reaction products might appear

  • housing: Fe, Cr and Ni reaction products may dissolve

Table 4 gives a selection of possible corrosion products. It is obvious that corrosion products pose rather greater hazards than the active materials. Many of them are corrosive and toxic, including to aqueous life, and some are even carcinogenic.

4.1.4 Ceramics. Binders and additives of ceramics are often AlPO4-based. The phosphorous can be reduced by certain alkali and earth alkaline metals to form metal phosphides. These may react with water to form highly toxic phosphine (PH3) gas, which is absorbed very fast in the lungs. Breathing such gas for 5 minutes at a concentration of 1000 ppm is lethal50,62,63. In certain cases, ceramic Al2O3 fibre material is used as a diaphragm. When entering the lungs, such fibres can cause cancer, with the probability being determined by the dose of exposure, dimensions of the fibres, and their biopersistence. Fibres with a diameter < 3 µm, a length > 5 µm and a length-to-diameter ratio of > 3:1 are considered carcinogenic64. Further, Al2O3 is considered very biopersistent, and therefore needs to be classified as carcinogenic cat. 1B50.

4.1.5 Recommendations. Battery safety can be increased significantly by avoiding BaCl2 and ceramics which contain AlPO4-based binders. When disassembling and cleaning cells, this work should only be performed in a fume hood while wearing gloves and eye protection. In case of accidents, the main exposure to toxic substances is probably via the lungs due to vapours, aerosols and possibly PH3. Further, hydrogen might be released. If it cannot be assured that the housing is hermetically sealed under all circumstances, the cells must be operated inside a fume hood to evacuate toxic or explosive gases3. Hydrogen traps need to be avoided3. Finally, a second crucible or absorption material around the cell might be useful to catch up spills65.

4.2 Electrical hazards

Typical electrical hazards include:

  • Short circuit: any fast discharge may lead to cell heating and pressure buildup, as explained in Section 4.5.5. Reasons for a short circuit might be abuse, a power outage, deposition of Na vapour on a feedthrough, internal self-discharge, Zn deposition or any other internal mutual metallic contact. Short circuits cannot be safely excluded.

  • Failure of pressure sensor: if used to monitor battery safety, the system should shut off if the pressure sensor fails.

  • Failure of heating system: if a thermocouple or heat controller breaks, the heating system must switch off. Thermocouples need to be fixed safely such that they cannot be removed accidentally. If necessary, a second heat controller for safety shutdown might be installed.

  • Overcharge or -discharge: too high or too low cell potentials may lead to current collector corrosion and salt decomposition. The latter may increase the internal pressure considerably, as explained in Section 4.5.4 and must absolutely be avoided. The corrosion potentials for various current collector materials are given in Table 16, the decomposition potentials of the salts in Table 14.

4.3 Thermal hazards

Thermal hazards include mainly

  • overheating, which might be caused by broken or removed thermocouples or failure of heat control

  • external fire, leading to overpressure and air corrosion as explained in Section 4.5.1 and Section 4.6.1

  • skin burns, which may happen if parts with a temperature above 55–65 °C are touched, as shown in Figure 5

4.4 Humidity and salt drying

Humidity is problematic because it may increase cell pressure and induce corrosion. Most salts are appreciably hygroscopic; the latter being defined as the ability of a material to take up water from the environment by adsorption, absorption or capillary action67,68. Effective procedures from drying salts are described in the foregoing. Good reviews on general approaches to salt drying are also available69,70.

The most typical reactions of water with chloride salts are the formation of69

  • hydrates, e.g. CaCl2 + H2O ⟶ CaCl2 · H2O,

  • hydroxides due to hydrolysis, e.g. ZnCl2 + 2 H2O ⟶ Zn(OH)2 + 2 HCl,

  • oxides due to hydrolysis, e.g. ZnCl2 + H2O ⟶ ZnO + 2 HCl and

  • hydroxides from oxides, e.g. CaO + H2O ⟶ Ca(OH)2,

which can lead to the formation of hydrogen and contamination of the melt with corrosive O2–, OH–, Cl– or H+ ions. The simplest approach to purifying salts is heating under vacuum. While slightly hydrated salts such as KCl and NaCl can easily be vacuum dried without precautions, care must be taken with others because of hydrolysis reactions71. Suitable drying temperatures are best obtained from thermogravimetric analysis (TGA) experiments, salt-water phase diagrams or other suitable literature. Salts which undergo hydrolysis should first be dried in vacuum at low temperature before rising it slowly69,70. In order to speed up the process regular purging with inert gas is recommended71,72. The achievable vacuum pressure is a measure of the success of the drying procedure.

b2580137-ff01-476a-bbbc-81dffecace91_figure5.gif

Figure 5.

Burn threshold of metals (a) and ceramics (b)66.

Salts for which hydrolysis cannot be avoided need to be melted under HCl, and HCl or Cl2 should be bubbled through this melt to remove oxides/hydroxides70,71. This approach does not eliminate the need for vacuum drying. Alternatively, sublimation or distillation may be used although they are rather costly70.

Barium chloride is hygroscopic and is stable as a dihydrate in contact with air50,59,73–76. The water-BaCl2 phase diagram77 predicts di-hydrate decomposition at 102 °C77–79, mono-hydrate decomposition at 145 °C77 and hemi-hydrate decomposition at 167 °C77,78 at ambient pressure; at 0.1 mbar it can even be fully dried at room temperature. TGA experiments show water loss between 60 and 150 °C; heating to 160 °C is claimed to be sufficient for drying80. The dehydration-rehydration process is claimed to be fully reversible81, but information on hydrolysis is limited82–84. At least above 900 °C, hydrolysis has been demonstrated experimentally83,85 and is also predicted by HSC41.

Calcium chloride is very hygroscopic50,59,74; its phase diagram has been investigated several times86–91. CaCl2 can exist as 1/3, mono-, di-, tetra- and hexahydrate50,92–95. Smith et al. give an excellent overview on drying CaCl296. At ambient pressure, CaCl2-hexahydrate reacts to tetra-, di- and anhydrate and liquid water at 3097, 45 and 175 °C59,73–75,98. However, the dehydration steps and phases depend much on pressure – and in certain cases higher temperature up to approx. 300 °C might be required94,99. Further, hydrolysis has occasionally been observed at 380 °C100,101 – and often at higher temperatures above 600 °C84,102–104. Such reactions produce CaO above 400–450 °C105,106; at lower temperature, Ca(OH)2 might be more stable. Purifying CaCl2 under vacuum for one week at 100 °C, followed by another week at 225 °C, leads to a contamination of 0.3 wt% H2O107, which is equivalent to a more sophisticated purging with HCl at 850 °C under vacuum.

Sodium chloride is only slightly hygroscopic74. While mined salt contains up to 0.4 wt% humidity, NaCl does not form hydrates but only adsorbs humidity on the surface96. Water-NaCl phase diagrams do exist but focus often on the NaCl-solubility49,88,108. Smith et al. thoroughly reviewed the drying procedure of NaCl suggesting that drying at 400 °C under vacuum leads to complete water removal96. Wang et al. found that NaCl contained initially 0.026 % humidity and that complete drying took approx. 12 h at 120 °C109. Hydrolysis of NaCl has been investigated repeatedly, and might occur at 450 °C. However, when dried under inert gas, it is considered negligible96,110–112.

Lithium chloride is extremely hygroscopic98,113. Although several hydrates are known, only the monohydrate is relevant as the others only occur below 0 °C113,114. Phase diagrams are given by various authors91,114–116 – see also the references therein. In contact with air, LiCl forms a surface layer of LiCl · H2O (2.55 % water)117. TGA measurements show that drying occurs in two steps between 99–110 and 160–186 °C118 or according to other authors at 80 °C and the rest between 96 and 175 °C80. Hydrolysis has been observed at 390–500 °C69,72,119, with increasing propensity near the melting point around 600 °C112,117,119,120. According to Smirnov et al., hydrolysis produces comparable amounts of oxide and hydroxide110. Drying has been shown to be a slow process: vacuum and flushing three times with inert gas needed 40 h at 25 °C, and 20 h at 100 °C to achieve a pressure of 133 Pa72. Swain et al. carefully reviewed possible drying procedures suggesting that heating to 300 and 500 °C for more than one week under vacuum yields similar purity as using HCl121. Other authors suggest based on TGA measurements a temperature of 450 °C under vacuum72 or 480 °C – 500 °C followed by fusion under vacuum and if possible under anhydrous HCl120 or Cl296.

Potassium chloride is only slightly hygroscopic, adsorbing water on its surface if humidity surpasses 66 % relative humidity96,98. Water-KCl phase diagrams are available49,88,122; a good overview on drying is provided by Smith et al.96. TGA measurements have shown that KCl looses water at 219 °C80,96. Hydrolysis can theoretically happen, and has been measured at temperatures as low as 500 °C. However, it is negligible if heated under protective gas72,110,111,123. According to Wang et al., KCl drying required 30 h at 120 °C to remove the 0.03 % water originally present. Typically, heating to 300–400 °C under vacuum with regular flushing with inert gas is the recommended drying procedure96.

Strontium chloride is hygroscopic, forming hexa-, di-, mono- and hemihydrates50,73,76,124,125 according to the phase diagram124,126. Dehydration under a humid atmosphere proceeds step wise from the hexa- to the di- to the mono-hydrate, from 61–320 °C98,127. The exact transformation temperatures depend very much on air moisture – which is the reason why many authors give different values126–128. In dry air, only the monohydrate is stable126 and forms the anhydrate at 37 °C126. Hydrolysis can be expected especially for the higher hydrates and higher temperature82,84 and has been shown to occur at 935 °C85.

Zinc chloride is the most practically challenging of all the salts considered. It is strongly hygroscopic50,75,95,98,129 and many hydrates are known, including 1.33, 2.5, 3 and 4.5-hydrate95,129–133. As can be seen in the phase diagram, dewatering happens in five steps95,130. All water is not removed until ZnCl2 is heated above its melting point; the last 0.1 % disappears above 310 °C and is fully lost at 350 °C130,134. Threlfall claim that ZnCl2 contains water even up to its boiling point135.

Hydrolysis of ZnCl2 has often been studied and is as complex as dehydration. It is well known that it depends on the exact salt mixture and that ZnO can limit HCl formation. Depending on the exact conditions, hydrolysis has been observed to set in at temperatures of 160–340 °C130,136–139. Giving a thorough overview on the purification of ZnCl2, Hamilton states that the degree of hydrolysis is low139. His drying procedure is similar to the one recommended by other authors140,141, and consists of: vacuum drying for 4–5 days until pressure decreases to 5 · 10−3 torr; heating to 250 °C for several days until the same pressure is obtained; flushing with HCl while heating to 350 °C; further bubbling with HCl for 5 h; and finally, flushing with dry Ar for 5 h.

Recommendations Salt drying is a mass transfer controlled process. A large surface area of the material, for example as powder, and regular flushing with inert gas is therefore useful. Drying should be performed under vacuum and for sufficient time – as rule of thumb for at least one day, but better a week. Salts should be dried separately, especially those where hydrolysis can be expected. The exact drying procedure, including heating speed and temperature steps, need to be adjusted for the specific salt – based on scientific information such as phase diagrams, TGA measurements or similar. Salts which tend to undergo hydrolysis are generally best predried at room temperature before increasing temperature slowly. In case of very challenging salts such as ZnCl2, purging of the melt with HCl or Cl2 might be required to remove all moisture.

4.5 Pressure buildup

Pressure buildup in LMBs can have different causes and may potentially be dangerous. The European Pressure Equipment Directive 2014/68/EU provides a regulatory framework to design safe pressure devices142. As the volume of our cell is below 1 l and the expected maximum pressure below 200 bar, it does not directly apply.

4.5.1 Heating. Pressure buildup during heating can be adequately approximated by the ideal gas law as40

pV=nRT(2)

with the temperature T in K, the amount of substance n, the gas constant R and cell volume V. As shown in Table 5, this may lead to an overpressure of 2 bar at normal operation. Even a temperature increase to 900 °C would add only one bar more.

Table 5. Overpressure due to heating.

T (°C)Δp (bar)
250
6001.9
7002.3
8002.6
9002.9

Figure 6 shows the measured cell pressure within a battery during heat-up. The slight pressure over-estimation can be attributed to the presence of the pressure-sensor tube (see Figure 3), which encloses a significant volume of gas with a lower temperature than the gas in the main body of the cell (tube dimensions: 300 mm length, 4 mm internal diameter). However, overall the experimental and theoretical curve match well, and do – most importantly – not show evidence of additional pressure increase due to humidity.

b2580137-ff01-476a-bbbc-81dffecace91_figure6.gif

Figure 6. Pressure rise predicted by the ideal gas law (black) and measured in a battery experiment (orange).

4.5.2 Vapour pressure. The vapour pressures of Na, Zn and ZnCl2 are considerable and lead to continuous evaporation in open cells – as shown exemplary in Figure 7. However, their contributions to the overall cell pressure can safely be neglected, as shown in Table 6.

b2580137-ff01-476a-bbbc-81dffecace91_figure7.gif

Figure 7. Na vapour forming at the anode of an open Na-Zn cell experiment.

Table 6. Vapour pressure of battery materials at 600 °C.

★ Emons et al.143 do not mention the unit of their vapour pressure equation; for plausibility reasons, torr was assumed. FactSage gives an order of magnitude smaller value of 3.1 · 10−7 Pa.

compoundvapour pressurecomment
Pabar
Ba7.17.1 · 10−5at melting point45
Ca2182.2 · 10−3at melting point45
K203140.245
Li7.47.4 · 10−545
Na33820.034144
Sr7.77.7 · 10−5145
Zn14890.01546
BaCl23.83.8 · 10−5at melting point146
CaCl20.0282.8 · 10−7at melting point147
KCl51.55.2 · 10−4at melting point70
LiCl3.93.9 · 10−5at melting point147
NaCl464.6 · 10−4at melting point147
SrCl20.484.8 · 10−6at melting point146,143★
ZnCl2160000.1670
H2O22 · 10−6 Pa220at critical temperature
of 374 °C39

4.5.3 Water, hydroxide and oxide decomposition. Humidity in the cell will result in hydrogen production thus increasing cell pressure. The exact amount of water depends on the cleaning of the battery parts, on the specific salt and its drying procedure. Especially ceramic parts can absorb water and should be carefully dried before use. Table 7 gives an overview of measured water contents in various salts after purification.

Table 7. Water content in purified salts.

saltwater contentpurification stepssource
CaCl20.3 wt%5–7 days at 100 °C, then 225 °C for 5–7 days under vacuum107
0.3 wt%850 °C under vacuum, sparging with HCl for 30 min, then Ar107
KCl0400 °C96
030 h at 120 °C109
LiCl0.17-0.4 mol%LiCl-KCl mixture heated for 1 h in vacuum to 480 °C119
NaCl0NaCl-KCl mixture heated to 700 °C under vacuum for 15 min119
ZnCl211.2 %120 °C, 32 h109

A water concentration of 0.3 wt% in CaCl2 can be assumed as realistic while NaCl might be assumed to be fully dry. After assembling a cell in a discharged state using Zn, NaCl and CaCl2, humidity might react slowly with Zn to form H2 and Zn(OH)2 as this is the stable species at room temperature – see Table 15. When heating the battery, the reaction might accelerate, forming ZnO instead of hydroxide above 85 °C41. During the first charge, water may alternatively react with ZnCl2 (by hydrolysis) or with Na to form NaOH.

To estimate the pressure increase due to hydrogen release, only the free space above the crucible – ignoring the feedthroughs, barrel connectors and small tube – is assumed as free gas volume as

V=π4d2h=π43.72⋅1.39=15cm3.(3)

Assuming that the CaCl2 contains 0.3 wt% water, the total water mass is m = 0.6 · 32 g · 0.003 = 0.058 g or n = 0.0032 mol. At 600 °C, the ideal gas law39,40

p=nRT/V(4)

predicts a pressure of 1 548 kPa = 15 bar for the water vapour alone assuming that all of the initial water’s hydrogen is released, and its oxygen forms oxides with negligible vapour pressure. Adding the thermal expansion of the Ar gas cushion results in a total pressure difference (between the capsule interior and normal atmospheric pressure) of almost 18 bar. Pressure measurements made on real experimental cells report values that are substantially lower than this, supporting the efficacy of the salt drying procedures described in Section 4.4.

Based on Table 15, it is impossible to predict which oxide or hydroxide will be formed preferentially at 600 °C. Comparing only the decomposition potentials, and assuming that the species with the highest potential is the most stable, the formation of Ca(OH)2 would be preferred. This might be true if Ca(OH)2 does not dissolve in the salt. However, if it dissociates into Ca2+ and OH– ions, the various hydroxides cannot be distinguished any more and hydroxide decomposition may occur much below the decomposition potential of Ca(OH)2. Moreover, complex ions, hydroxychloride or other compounds might be formed139,148.

Under these circumstances, and also considering that the decomposition potentials in Table 15 do not account for activities, it cannot be predicted at which potentials gas evolution will start. It is, however, obvious that especially oxygen would immediately back-react with any metal to oxide in closed cells. Similarly, hydrogen may back-react with oxides to hydroxides if these are more stable. The full release of all bound hydrogen can therefore be considered as the worst case scenario. In any case, oxides and humidity must absolutely be avoided as their decomposition and reaction with the cell’s electroactive materials might significantly reduce its coulombic efficiency.

4.5.4 Salt decomposition. If excessively low or high inter-electrode potentials are applied to the cell the electrolyte might decompose to form metal and chlorine gas. As a worst-case scenario, 12.8 g (0.219 mol) of NaCl and 19.2 g (0.173 mol) of CaCl2, fully decomposed, would result in 0.28 mol of chlorine gas. Taking a simplified large cell volume of

V=π4d2h=π43.12⋅6=45cm3(5)

this corresponds to a cell pressure of

p=nRT/V≈450bar.(6)

Table 14 gives an overview of theoretical decomposition potentials, neglecting the species’ activities. It should be emphasised that the chlorine evolution reaction will compete with the Zn oxidation reaction at charge, or with the anode current collector corrosion reaction at discharge. Gas generation might therefore be slow. Moreover, chlorine is expected to back-react immediately with any metal in the cell so that it is unlikely that large amounts of chlorine can be generated.

The attentive reader might notice that the decomposition potential of ZnCl2 is with 1.6 V lower than the cell’s open-circuit potential. For decomposition to occur, Zn2+ ions need to reach the anode current collector. However, this is impossible because they will immediately be reduced by (dissolved) Na when "approaching" the anode. ZnCl2 decomposition is therefore only possible if building cells containing ZnCl2 in discharged state, or when (much) Na is lost during cell operation. However, care must be taken to cycle within predetermined safe potential limits.

4.5.5 Short circuit. An instantaneous adiabatic full-cell discharge is the worst conceivable outcome of a short-circuit. The resulting temperature increase can be calculated as follows.

The extent of the reaction is limited by the amount of available Na. Assuming that the battery is charged until salt solidification (DoD = 45 %) and that the complete salt column (i.e. not just the salt below the diaphragm) participates in the reaction, the amount of Na is

n=mM=0.4⋅32g⋅0.4558.44g/mol=0.1mol,(7)

where m denotes the mass and M the molar mass of Na.

The enthalpy change of the cell reaction (Equation 1) can be expressed as149

ΔH=2⋅H(NaCl)+H(Zn)−H(ZnCl2)−2⋅H(Na).(8)

As simplification we neglected the enthalpy of mixing of NaCl/ZnCl2 with molten CaCl2 and simply extrapolate the enthalpy of formation of liquid NaCl to 600 °C and assume an ideal solution. Such an approach is justified as the enthalpy of mixing in NaCl-CaCl2 systems (< 3 kJ/mol,150) and NaCl-ZnCl2 systems (< 8 kJ/mol,151) indeed is small. Using the values of Table 8, the total enthalpy liberated by the reaction is then given as

Q=−n⋅ΔH=36.5kJ.(9)

Table 8. Enthalpies of formation of Na, Zn and their chlorides at 600 °C.

compoundH (J/mol)source
Na(l)1985341
ZnCl2(l)-356844152
NaCl(l)-352778152
Zn(l)2382841

Considering that all ZnCl2 disappears during the reaction, metallic Zn (being the most volatile constituent) would be the first to evaporate when reaching 907 °C – see Table 10. With the heat capacity of the active materials of 45.9 J/K according to Table 9 the necessary heating would consume

Q=(907K−600K)⋅45.9J/K=14.1kJ,(10)

Table 9. Mass, molar mass, amount and heat capacities of Na, NaCl and ZnCl2.

mMncpsource
gg/molmolJ/mol KJ/K
Zn2565.390.382331.412.00153
NaCl12.858.4430.219067.914.87154
CaCl219.2110.9830.173011019.03154
sum45.9

Table 10. Boiling points of Zn and the salts.

Tb (°C)source
Zn90745
BaCl2156075
CaCl21936155
KCl150075
LiCl136075
NaCl1465155
SrCl2125075
ZnCl273275

which means that 22.4 kJ are left for evaporation.

In order to evaporate all Zn, an energy of 44 kJ would be required, considering that the heat of evaporation of Zn is 115 kJ/mol45. Therefore, roughly 50 % of the Zn might evaporate. Assuming ideal gas behaviour and using only the free volume above the crucible (Equation 3) the resulting pressure increase would amount to 1 bar, as shown in Table 5.

4.5.6 Recommendations. Table 11 summarises reasons and values for pressure increases. Obviously, it is imperative to avoid salt decomposition due to overcharge or overdischarge. Further, it is very important to carefully dry the salts, because even small quantities of residual moisture might lead to pressure buildup on the order of 18 bar. When using new salts or trialling new charging currents, a pressure monitoring is recommended. If all recommendations are followed, normal cell overpressure will be on the order of 2 bar.

Table 11. Possible pressure increase in the cells due to various effects.

effectpressure
increase (bar)
comment
vapour pressure0.2by ZnCl2, Zn and Na
heating2
short-circuit1
water18assuming 0.3 wt%
water in CaCl2
salt decomposition450
overheating1if 300 K more

4.6 Durability of housing

The cell housing protects the environment from the cell’s hazardous constituents, and the cell interior from moisture and oxygen. Its long-term integrity is therefore essential. The choice of materials, design and calculations are explained in Section 6.4. In the following, possible cell failure mechanisms will be discussed.

4.6.1 Corrosion. Na is able to reduce most other metals and might therefore attack ceramics, such as the Al2O3 of the feedthrough; this depends of course on temperature156. Further, it might dissolve Ag from the braze of the feedthrough in the event that sufficient amounts of Na condense there157. Steel and other metals will also be attacked by HCl, which is formed due to hydrolysis caused by humidity of the salts. While pure salts are not corrosive, impurities such as O2, H2, H+, H2O or OH– can act as oxidising agents and can lead to rapid corrosion. If the gas-tight seal is broken, then a continuous inflow of the surrounding atmosphere can be expected. In such case a rapid corrosion of the housing is inevitable, as demonstrated in Figure 8 (a). In this example, the cell was not tightened on purpose. In a short time (ca. 6 h), the corrosive salt has destroyed the housing. Liquid Zn, which will – like Na – evaporate and condensate at different places within the cell housing, is able to easily dissolve steels158–160. An example of a Zn dissolved Inconel barrel connector is shown in Figure 8 (b). Finally, excessively high potentials might lead to electrochemical corrosion, if there is electrical contact with the part in question. Overall, an extensive cell testing and thorough understanding is necessary to be able to safely exclude internal corrosion of the cell.

b2580137-ff01-476a-bbbc-81dffecace91_figure8.gif

Figure 8.

Corrosion of an untight cell body due to leaked molten salts in (a), corrosion of an Inconel barrel connector due to Zn vapours in (b), failure of a small feedthrough due to high temperature and increased pressure in (c) and material sedimentation on internal parts leading to compositional changes and eventual failure of the cell due to high resistance in (d).

The cell might not only fail due to corrosion from the inside, but also due to attack from the outside. For example, certain insulation wools contain chloride ions which are able to attack steel161–163. Further, HCl vapour in chemical laboratories will have a similar effect. Maybe most importantly, the feedthrough braze is usually not stable in air and will corrode slowly. According to the manufacturer, simple Ag-Cu brazes can only be used up to 350 °C in air, while Au-covered brazes might be used up to 450 °C164. A failure of a small feedthrough as well as corrosion of larger Ag-Cu ones are shown in Figure 8 (c).

4.6.2 Thermal shock and stresses. Volume change and thermal stresses are extremely important for cell safety. Rapid heating or cooling is especially harmful for ceramics as they conduct heat slowly and the resulting differential stresses might lead to cracking165. The heating/cooling rate must therefore be limited to 5 K/min166. Moreover, volume change is a significant challenge as some salts expand by 20–30 % upon melting – see Table 12. Zn, which melts more than 100 K earlier than the salt might be trapped in the salt and exert strong forces on its surroundings. While the battery housing has been shown to be able to cope with these stresses, the sealing of the feedthroughs might nonetheless be damaged.

Table 12. Melting points (Tm), densities (ρ) and volume change of metals and salts defined as ΔV/V = (Vhot – Vcold)/Vcold = ρcold/ρhot – 1.

If no reference is given, the volume change has been calculated. ★ In computing the volume change of the metals, the volumetric expansion coefficient has been assumed to be 3 times the linear expansion coefficient.

substanceTmρ (g/cm3)volume change (%)
25 °CTm (lq)600 °Csolidmeltingliquid
Ca839591.54401.37840-440★7.4★-
84240
Na98400.97400.927153,1680.808153,1681.640★2.616914.7
Zn420407.14406.57445,466.398453.840★4.081692.75
BaCl296240,59,75,983.85673,75
3.9198
3.174403.7084943.570-
CaCl2772752.15752.085402.0914940.0970-
775402.17449
KCl770591.984751.527401.832498.317–2370,170-
77140,981.98798
LiCl605752.06875,981.502401.891499.426.2170-
61040
61498
NaCl801402.165751.556401.990498.823–3070,170-
SrCl2874403.05275,982.727402.892495.52.4–4.270-
87598
ZnCl2283982.90775,982.54402.89249311.6705.849
29040,752.9849(at m.p.)
CaCl2-NaCl 44:56 mol%~530492.17491.94471.91475.1495.1491.57

4.6.3 Manufacturing defects and ageing. Weldseams can always contain defects. Although many material tests are available167, a simple pressure test of the vessel might be the most reasonable approach to defect identification. It would also ensure that compression fittings are correctly mounted when using a pressure sensor or thermocouple. Finally, a torque wrench should be used to tighten the screws and hermetically seal the cell.

Battery ageing may be caused by any corrosion process, but also by microstructural changes in the steel from which the housing/screws are made. For example, a very brittle Fe-Cr phase might form between 600 and 800 °C if the battery is exposed to this temperature for several hours. This sigma phase can appear only in steels with a minimum Cr content of 18–20 %, where Si, Mn, and Mo promote sigma phase formation167. As the 1.4980 steel (used here for screws) has a chromium concentration of 13.5–16 %, and the 1.4306 steel (used for the housing) has chromium concentration of 18–20 %, sigma phase formation is theoretically possible only for the housing.

Secondly, at 475 °C embrittlement can be expected in ferritic Cr-steels if held for several hours between a temperature of 400 and 550 °C167. Fortunately, this is rather improbable as the Na-Zn cell operates at higher temperature and both of the steels used are austenitic.

Finally, electrolyte ageing might be a challenge, too. As shown in Figure 8 (d), during the 400 h electrochemical cycling experiment, salt has gradually deposited on the ceramic walls, irreversibly altering the remaining composition. This eventually leads to increased resistance and higher potentials.

4.6.4 Abuse. Several possibilities exist for abuse of Na-Zn cells. Physical impacts, thermal shocks, and exposure to corrosive substances, among others, must be excluded. During disassembly, cells must be handled carefully, especially when removing their lids to avoid damage to the flange’s knife-edge and/or sealing surface. The feedthroughs and pressure sensor tube in the lid are both fragile and should be handled with the necessary care. Cells should not be lifted using the pressure sensor tube.

4.6.5 Recommendations. Designing a cell housing which can safely contain the active materials under all probable circumstances is very challenging. As explained in Section 6.4 it is especially difficult to calculate the appropriate tightness of the screws at 600 °C, as well as an appropriate feedthrough design.

Cell pressures in the order of 2–3 bar during normal operation can safely be contained using the materials investigated to date (see Table 2). However, traces of moisture might induce considerable overpressure on the order of 18 bar. In such scenarios, the housing, tube and screws are still expected to maintain their integrity – most probably the braze of the feedthrough will fail first. The pressure sensor might also fail at such high pressures. Finally, volume changes leading to deformation of the current collector and stresses in the braze of the feedthrough can easily destroy the latter. Concerning long-term stability, the feedthroughs and their corrosion by air is clearly the limiting factor. Corrosion from inside is probably less problematic as long as the cell is properly sealed.

To ensure safe operation, the following safety measures are recommended:

  • battery prototypes should always be operated under a fume hood as the sealing might fail at any time

  • only carefully dried salts should be used

  • when using new salt mixtures, the cell pressure should be monitored

  • standard procedures for drying, filling and assembling (torque, etc.) should be developed

  • all cell prototypes need to be handled with care

5 Conclusions

A safety assessment of a Na-Zn Liquid Metal Battery (LMB) has been performed at the cell level with a focus on operation in a laboratory furnace. Material, electrical, thermal and mechanical hazards have been discussed. It has been shown that safety of Na-Zn LMBs depends crucially on the selection of a safe electrolyte; if technically possible, avoidance of LiCl and BaCl2 is desirable. One of the main hazards, cell overpressure, can be avoided by proper salt purification and by operating the cell in a safe potential window, as is the case for ZEBRA, Na-S and AMBRI’s Ca-Sb batteries. In terms of cell engineering, LMBs are still at a low TRL level and certain aspects of their potential failures modes are not yet fully understood. However, it can be predicted at the outset that LMBs can reach a very high safety level, similar to ZEBRA batteries, because they are not vulnerable to thermal runaway. In this important respect, the cells are safer than Na-S or Li-ion batteries, and are expected to comply with the (relatively demanding) safety standard UL 9540A32 in future.

To further improve cell safety, a better understanding of corrosion mechanisms and corrosion products is required. The weakest components of the cell housing are the feedthroughs; here, much knowledge regarding (air-induced) corrosion, thermal stresses, and mechanical durability is missing. Finally, the extensive topic of cell design and engineering has scarcely been covered in the past and requires more attention in future. Apparently simple phenomena, like the volume change of the salt upon solidification, or thermal stresses borne by the cell housing, are crucial to operate Na-Zn cells safely and efficiently at 600 °C, but are insufficiently well understood at present. In the face of these knowledge gaps, LMB prototypes should be operated under a fume hood until the various possible failure mechanisms are fully understood. Nevertheless, continuous operation of gas-tight batteries for up to 6 weeks outside a protective environment has demonstrated that this demanding but affordable energy storage concept not only has great potential, but may also become inherently safe in the near future28.

6 Tables and technical design specifications

6.1 Safety tests for batteries

Table 13. Typical safety tests for battery cells according to various standards29,31,32,171,172.

For the various misuse tests, noncompliant results are, e.g. leakage, fire, explosion, release of toxic or flammable gases.

testdescription
electrical tests
overchargea battery is charged to 110 %
high rate chargea battery is charged with 120 % of the specified maximal
current
short circuita charged battery is short-circuited with max. 20 mΩ
overload under
discharge
a charged battery is discharged once with 90 % of the rated
overcurrent protection value of the BMS, and once with 135 %
of the main fuse rating
overdischarge protectiona charged battery is discharged with the specified maximum current until the temperature/voltage protection of the BMS switches it off
temperature and operating limitsa battery is brought to specified upper temperature limit, then charged and discharged
imbalanced chargingall cells are fully discharged, while one is brought to a SoC of 50 %; then all together are charged with maximum current
insulation resistancethe electrical spacing and insulation are tested
continuity testthe grounding of the battery is tested
failure thermal managementthe battery is discharged, the thermal management system switched off and the battery charged with maximum current; the same is done with discharge
working voltage measurementsthe potential between live parts and metal enclosure is measured and compared with specifications
locked-rotor testthe fan of a possible cooling motor is blocked for 7 h
input currentthe input current drawn by accessory devices which are connected to AC is measured
leakage currentthe leakage current of AC secondary components is measured
strain reliefthe strain relief of the power cord is tested
push-back reliefit is determined whether the power cord can be pushed back into the device
low voltage transformera possible transformer is tested for fire hazards
electromagnetic immunity tests
electrostatic dischargetest for electrostatic contact discharge of 6 kV and air discharge of 8 kV
radio-frequency electromag. fieldimmunity against radio frequency is tested with 10 V/m from 80 MHz to 1 GHz and 3 V/m from 1.4 to 6 GHz
burst immunityimmunity to electrical fast transients/bursts is tested
impulse voltage testsurges of 0.5-2 kV line-to-ground are tested which might result from lightning
radio-frequency common moderadio-frequency conducted disturbances are tested at in- and output ports
power frequency magnetic fieldimmunity to 10 A/m power-frequency magnetic fields is tested
mechanical tests
vibrationa fully charged battery is subject to random vibration
shocka fully charged battery is subject to shock
crushbattery crushed between a fixed surface and a ribbed test platen
static force250 N are applied on all sides at a round 30 mm surface
impacta charged battery receives three impacts of 6.8 J
drop impacta charged battery is dropped depending on its weight up to 1 m
wall mount fixturean additional force of 3 times the weight of the battery is applied
hydrostatic pressure testcell needs to support 1.5 times its hydrostatic pressure
pneumatic strength testscell needs to support 1.3 times its design pressure
environmental tests
thermal cyclingenvironment temperature of a fully charged battery is changed between -40 and 75 °C
resistance to moisturetest of IP rating
salt foga salt fog test is performed for batteries to be installed near the sea
external fire exposurea fully charged battery is subjected to a fire for 20 min and should not explode
tolerance to internal cell failure test
single cell failure tolerancea failing single cell should not lead to destruction of the complete battery
thermal runaway test
cell levela single charged cell is heated at 4–7 K/min; if thermal runaway occurs or flammable gas is released, module test follows
module levelone or several cells in a module are forced into thermal runaway to observe propagation; if thermal runaway cannot be contained in module or flammable gas is released, unit level test follows
unit levelthe complete BESS is tested accounting for its installation site (indoor, outdoor)

6.2 Risk assessment table

b2580137-ff01-476a-bbbc-81dffecace91_figure9.gif

Figure 9. Excel table of the risk assessment.

6.3 Decomposition and corrosion potentials

Decomposition potentials for many pure substances have been tabulated, and are readily available in the literature. In general, these have either been measured experimentally, or calculated from thermodynamic data (specifically, the Free energy changes of their decomposition reactions). Table 14 and Table 15 summarise such data for substances relevant to Na-Zn cells. These are substances that are either components of a prospective electrolyte, or occur as contaminants in the cell.

Table 14. Decomposition potentials of chloride salts at 600 °C.

At overcharge, metal is produced on top and gas on the bottom of the cell, at overdischarge (negative potentials) inversely. Activities have been neglected.

saltΔE (V)
3641
BaCl23.73.7
CaCl23.53.4
KCl3.73.7
LiCl3.63.5
NaCl3.43.4
SrCl23.63.6
ZnCl21.61.5

Table 15. Decomposition potentials for oxides and hydroxides at 600 °C41, and stability of species.

At overcharge, metal is deposited on top, and gas released on bottom of the cell, at overdischarge (negative potentials) inversely. The ‘stable species’ entries are based on thermodynamic calculation neglecting activities and ignoring peroxides, superoxides and hydroxychlorides; the values should therefore be treated with care.

substanceproduct△E (V)stable speciescomment
25 °C600 °C
BaO
Ba(OH)2
Ba, O2
H2, O2
H2O, O2
BaO, H2O
2.4
3.6
2.6




hydroxide




hydroxide



BaO forms at 900 °C83
CaO
Ca(OH)2
Ca, O2
H2, O2
H2O, O2
CaO, H2O
2.8
3.80
2.76




hydroxide




oxide
2.2 V at 1000 °C175



stability limit hydroxide is 400 °C101,106
K2O
KOH
K, O2
H2, O2
H2O, O2
K2O, H2
1.2
3.1
2.1




hydroxide




hydroxide




KOH produced at 827 °C110; K2O2 might be more
stable at 450 °C69
Li2O
LiOH
Li, O2
H2, O2
H2O, O2
Li2O, H2
2.5
3.6
2.6




hydroxide




hydroxide




LiOH and Li2O appear in comparable amount110;
Li2O generation starting at ∼250 °C176
Na2O
NaOH
Na, O2
H2, O2
H2O, O2
Na2O, H2O
1.5
3.1
2.1




hydroxide




hydroxide
1.76-2.18175



NaOH produced at 450, 70096 and 827 °C110
SrO
Sr(OH)2
Sr, O2
H2, O2
H2O, O2
SrO, H2
2.6
3.7
2.7




hydroxide




hydroxide
ZnO
Zn(OH)2
Zn, O2
H2, O2
H2O, O2
ZnO, H2O
1.3
2.0
0.9




hydroxide




oxide
1.24-1.3 V175



hydroxychlorozinc might be formed instead139;
ZnO at least above 200 °C134

Table 16. Selected potentials for corrosion of current collectors.

cell∆E (V)comment
3641
Corrosion of anode current collector if going below
Al-Zn0.550.31first value at 200 °C
Co-Zn-0.47-0.50 
Cr-Zn-0.08-0.06Cr2+
Cr-Zn-0.29-0.31Cr3+
Cu-Zn-0.55-0.53Cu+
Cu-Zn-1.05-1.01Cu2+
Fe-Zn-0.35-0.31Fe2+
Fe-Zn-0.54-0.68Fe3+, first value at 350 °C
Mn-Zn0.350.39 
Mo-Zn-1.08-0.69Mo2+
Mo-Zn-1.03-0.63Mo3+, first value at 350 °C
Mo-Zn-0.97-0.78Mo4+, first value at 200 °C
Ni-Zn-0.55-0.61 
Ti-Zn0.330.41Ti2+
Ti-Zn0.280.33Ti3+, first value at 500 °C
W-Zn-1.16-0.71W2+
W-Zn-1.12-0.97 W4+
W-Zn-1.16-1.04W5+
W-Zn-1.23-1.10W6+
Corrosion of cathode current collector if going above
Na-Al1.331.60
Na-Co2.352.42
Na-Cr1.951.97Cr2+
Na-Cr2.162.23Cr3+
Na-Cu2.422.44Cu+
Na-Cu2.922.93Cu2+
Na-Fe2.222.22Fe2+
Na-Fe2.412.60Fe3+, first value at 350 °C
Na-Mn1.521.52
Na-Mo2.952.60Mo2+
Na-Mo2.912.54Mo3+, first value at 350 °C
Na-Mo2.842.69Mo4+, first value at 200 °C
Na-Ni2.42.52
Na-Ti1.541.50Ti2+
Na-Ti1.591.58Ti3+, first value at 500 °C
Na-W3.02.62W2+
Na-W2.992.89W4+
Na-W3.032.96W5+
Na-W3.103.02W6+

An important caveat to the use of these tabulated values is that they are strictly valid only for pure substances, whereas a Na-Zn electrolyte comprises a solution of several substances whose components’ activities may differ from their molar concentrations (i.e. exhibit non-ideal behaviour). The influence of such non-ideality on the potential is expressed by the Nernst equation, which, for a generic oxidation reaction at a single interface173,174 is

E=E0+RTzFln⁡aoxared(11)

where E0 denotes the standard potential (provided by the tables), R the gas constant, F the Faraday constant, T the temperature in K, z the number of exchanged electrons, and aox and ared the activities of the oxidised and reduced species respectively. The overall (inter-electrode) cell potential comprises the difference between two such interfaces

ΔE=Ec−Ea(12)

where the index a refers to the anode and c to the cathode. Thus, for the whole cell we have:

ΔE=E0,c−E0,a+RTzcF(ln⁡aox,c−ln⁡ared,c)+RTzaF(−ln⁡aox,a+ln⁡ared,a).(13)

Evaluation of activities is non-trivial, since there is no completely general model that successfully predicts their relationship to molar concentration, and experimental measurements on halide solutions are not comprehensive. By providing only the standard state terms (E0,c and E0,a), the tabulated potentials offer an approximation rather than a precise description of these decomposition potentials.

The cell potential at which one of the current-collector metals can oxidise – here termed the ‘corrosion potential’ – is a similarly important limit for sustainable cell operation. Table 16 displays such potentials for a range of candidate current collector metals. The metal couples in the left-hand column indicate possible exchange reactions: anode current collector versus Zn in the upper half; Na versus the cathode current collector on the lower half. The voltages displayed are those at which each metal couple undergoes electron exchange, resulting in the dissolution of the current collector metal into the electrolyte. For a pure single-component electrolyte, comprising the chloride of the reducing metal, such voltages are simply equal to the difference between the decomposition potentials of the chlorides of the metals concerned, according to Equation 12 above. However, as with the aforementioned decomposition potentials, the precise voltage for the multi-component case constituted by a Na-Zn cell, the activities of the components must be included in the calculation (Equation 13). Accordingly, Table 16 offers useful approximations rather than precise values.

6.4 Design and durability of cell

The details, calculations and further considerations concerning the cell design are summarised in this section.

6.4.1 Housing material. The steel for the cell housing needs to fulfil the following criteria:

  • heat-resistance: the steel needs to maintain high strength and structural integrity when subjected to 600 °C for long periods of time

  • scaling resistance: the steel needs to exhibit significant resistance to scaling, which refers to the formation of oxide layers on the surface when exposed to high temperatures in the presence of air

  • long-term stability at high temperature: material degradation or structural weakening at high-temperature during long time periods needs to be prevented

  • corrosion resistance: the steel needs to support the specific environment within the cell, including molten salt, Na and Zn vapour

  • adequate performance under thermal changes: the material needs to support large and repeated temperature changes including expansion and contraction

  • compatibility with other cell components: the steel is required to be compatible with other materials used in the cell avoiding any adverse reactions, material incompatibilities or degradation

  • manufacturing reliability: the selected steel must be consistently manufactured to precise specifications, to ensure reliability and avoid variations in material performance that could pose risks during cell operation

  • weldability, if possible without pre- or postheating

  • adequate machinability for easy manufacturing

Given the number of steels available in the market, it is impossible to provide clear advice how to select the most appropriate steel in a systematic manner. Even though patents of the LMB company AMBRI177 mention 1.4016 (AISI 430)178 to the best of our knowledge no study on suitable steels for LMBs has been published. We assume therefore that such steels which are used at high temperature for furnaces and in the chemical industry might be suitable. This includes in particular creep resistant, high-temperature steels. Table 17 provides a selection of steel grades which we consider to be suitable for LMBs.

Table 17. Possible steels and Ni-based alloys for high-temperature batteries with an operation temperature of 600 °C.

Data taken from various material data sheets and Wegst & Wegst181.

materialcharacteristics
1.4762
X10CrAlSi25
AISI 446
Ferritic stainless steel of low strength but excellent resistance to high-temperature oxidation. Weldable, but might need pre-heating. Application: industrial furnaces, combustion chambers, oil burners, heat exchangers, kiln liners, glass moulds.
1.4828
X15CrNiSi20-12
AISI 309
Standard steel in furnace building of high strength and corrosion resistance up to 650 °C in air. Weldable without preheating. Application: annealing bells, cementation and hardening boxes, annealing pots, etc. Alternatives: 1.4835, 1.4841.
1.4845
X15CrNi25-21
AISI 310S
Austenitic steel with corrosion resistance in air up to 1050 °C. Weldable. Applications: furnace building, chemical industry, steam boilers, petroleum processing plants, heat treatment baskets, etc.
1.4864
X12NiCrSi35-16
AISI 330
High strength and corrosion resistance in air up to 1000 °C. Welding without pre-heating. Applications: furnace building, chemical industry, heat exchangers.
1.4876
X10NiCrAITi32-20
Alloy 800
High-temperature strength and excellent resistance to oxidation up to 1100 °C in air. Weldable. Applications: parts for furnace and steam boiler constructions, petroleum industry, heat exchangers, and furnace components. Similar alternatives: 1.4958 and 1.4959.
1.4910
X3CrNiMoBN17-13-3
AISI 316LN
Creep-resistant alloy for usage up to 700 °C. Weldable. Application: pressure vessels, steam boilers, chemical industry.
1.4922
X20CrMoV11-1
Creep resistant construction steel for usage in air up to 600 °C. Low corrosion resistance due to low Cr content. Application: chemical industry.
2.4816
NiCr15Fe
Alloy 600
Ni-bases superalloy with excellent corrosion resistance up to 1050 °C. Weldable. Applications: industrial furnaces, chemical industry, reactors, aerospace applications.
2.4856
NiCr22Mo9Nb
Alloy 625
High-temperature alloy for use up to 1050 °C with excellent corrosion resistance. Weldable without preheating. Applications: chemical process industry, offshore and environmental technology.

As standard vacuum parts for our cell design were not available in the steel grades mentioned, simple 1.4306 had to be used for the housing and lid. At temperatures exceeding 500 °C, creeping will always occur179. We therefore base the strength calculations on the assumption that a deformation of 1 % in 10 000 h (Rp1.0) is acceptable179. Table 18 provides the material properties.

Table 18. Material properties of steel 1.4306 with data taken from various data sheets.

propertyunitvaluecomment
maximum use temperatureTmax°C600
yield strengthRp0.2N/mm290
yield strengthRp01.0 (10 000 h)N/mm2138for the similar 1.4307179
thermal expansion coefficientα1/K18 · 10−6

6.4.2 Housing cylinder. The allowed pressure within the cell housing, as dictated by its material properties, can be calculated as180

pal=2Rp1.0SdaS=2⋅138⋅1.540⋅1.5=69bar(14)

with Rp1.0 denoting the yield stress and S = 1.5 the safety factor179,180. The wall thickness is s = 1.5 mm and the outer diameter da = 40 mm. As the cells will only be pressurised up to 2 bar under normal operation, the housing is safely dimensioned.

6.4.3 Tube. The tube extending through the lid capping the cell serves to connect a pressure sensor, thermocouple or similar. Using the same formula for cylindrical pressure vessels as for the cell housing, an outer diameter of 6 mm and a wall thickness 1 mm yields

pal=2Rp1.0SdaS=2⋅138⋅16⋅1.5=307bar,(15)

which is, as previous, more than sufficient to contain the expected operating pressures.

6.4.4 Compression fittings. Compression fittings are used to attach a pressure sensor, bursting disk or thermocouple to the tube. According to the manual, for a 6 mm tube, a minimum wall thickness of 0.8 mm is required182. With a temperature reduction factor of 0.49 for AISI 304L (1.4306), the tube would support 211 bar at 600 °C. Most probably, it can be safely assumed that the fittings are designed for the same pressure.

6.4.5 Pressure sensor. Pressure sensors are sometimes used to monitor the cell pressure during heating and to detect leaks in the housing. According to the data sheet, they support 2.5 times the pressure of their full scale183. The typically used 4 bar sensors can therefore only support 10 bar before they might fail.

6.4.6 Welding. The housing is TIG welded by butt joints between bottom plate and the tube, and between the tube and the flange. As these weldseams are rather thick compared to the 1.5 mm tube, no failure is expected here.

The tube in the lid as well as the feedthroughs are laser welded in order to prevent damage from the feedthroughs. As the gap between laser welded parts needs to stay below 10 % of its wall thickness, and the feedthrough tubes are only 0.5 mm thick, a maximum gap width of 0.05 mm, i.e. very narrow tolerances are required for successful welding167. The final weldseam is usually 1 mm wide, with its depth depending on welding speed – possibly reaching 1–5 mm167. Obviously an accurate machining of the parts is necessary to meet the required tolerances. As the laser welding might be imperfect, a pressure test is recommended. Laser-welded parts should be handled with care.

6.4.7 Screws and Cu sealing. The lid of the cell is fixed with six M6 screws (ISO 4017, 1.4980). The latter need to deform the Cu sealing ring sufficiently to ensure the formation of a gas-tight seal, and need to be tightened such that they do not unfasten themselves while heating. However they also need to be removable after battery cycling. Finally, they should support an internal cell pressure of 18 bar, as explained in Section 4.5.6.

The correct dimensioning of screws starts by calculation of the preload force, accounting for cell pressure, deformation of the sealing, surface pressure and deformation of parts. Knowing the required force of the screw, the torque can be calculated. Finally, the static strength, surface pressure and sealing tightness safety factors are assessed184. This stress analysis involves several empirical formulae, which are well established for room temperature. However, when heating the cell to 600 °C, material properties such as yield strength or elastic modulus, among others, will change. Creeping of parts will occur, since the screw, housing and Cu have different thermal expansion coefficients, as well as being subject to a temperature gradient between the hot capsule interior and the colder exterior184,185. Although it is very challenging to correctly design the screws under such conditions, some general statements can be made. The high-temperature material (1.4980), with its yield strength of Rp0.2 = 380 N/mm2 at 650 °C186, allows for a force of 5 880 N in each screw. This is remarkable as an internal cell pressure of 18 bar would lead only to ca. 360 N. Under some assumptions, a force of 4.5 kN per screw is required for a sufficient deformation of the sealing ring and 3 kN to keep the seal tight over time. Tightening the screws with 100 % of its yield strength would lead to 6 Nm – which is a very small value compared to typical torques for M6 at room temperature of 7.7 - 26.8 Nm185. As the cell housing made of 1.4306 has a lower strength, the surface pressure of order 210 N/mm2 might be a problem.

Experimental trials have shown that a tightening torque of 5 Nm was not sufficient for proper sealing, and 10 Nm was hard to loosen again after a long-term cycling. Therefore, 8 Nm was identified as the appropriate average value to keep the cells gas-tight during normal cycling experiments. This is consistent with the calculated 6 Nm – which should still be sufficient for the screws to support an internal cell pressure of 18 bar.

6.4.8 Feedthrough. The approximate dimensions of the feedthroughs used, which are acquired from Kyocera164,166 or Alumina Systems, are shown in Figure 10. Typically, the insulator is made of Al2O3, the collars of Invar 42 (1.3917) and the conductor of Ni. Brazing between the ceramic and metal, as well as between the conductor and the collar is performed either with eutectic Ag-Cu braze (melting point 780 °C) or Au-Ni braze (melting point 950 °C)164,166. While the Ag-Cu braze is comparably cheap, it clearly reaches its limits at 600 °C – especially with small but rapid changes in temperature, the sealing will fail28.

b2580137-ff01-476a-bbbc-81dffecace91_figure10.gif

Figure 10. Dimensions of the Kyocera/Friatec feedthrough.

The values in brackets are estimated from the image in the manufacturers catalogue164.

A correct stress analysis of the feedthrough is challenging187. It must involve the strength of the ceramic, the thin Invar 42 collars and the three brazing points. While Invar 42 yield strengths48 are available at 600 °C, values for the brazes are scarce188. Apart from the internal cell pressure, forces may act via the current collector on the pin due to different thermal expansion – as explained in Section 4.6.2. The stress conditions will be complex, and might be better addressed with FEM simulations. Applying a lateral force by, for example, attaching an off-centred current collector will add an additional strain on the braze joint. Finally, also long-term stability of materials is a challenge since the parts of the feedthroughs are susceptible to various corrosive vapours187, e.g. Na attacks the ceramics as well as the braze while the conductive pin and collars could alloy with Zn. Cheaper Ag-Cu brazed devices are at 600 °C at their limit, and even Au-Ni brazed versions might fail if safe handling is not ensured and correct operational parameters, such as low heating/cooling rates, are not set. Overall, the sealing of the feedthrough is clearly the weakest point of the cell housing. Therefore, it is worthwhile to focus actively on improving the durability of the feedthroughs and investigating the various failure mechanisms in detail, both experimentally and numerically.

Data availability

Underlying data

The risk assessment table and selected calculations are available under the terms of the Creative Commons Attribution 4.0 International license (CC-BY 4.0)189.

Acknowledgements

We thank the SOLSTICE consortium and especially Bernd Willers, Camilla Sommerseth, Ole Kjos, Cathrine Solem, Marta Navas, Milena Salvo and Bjarte Øye for support and helpful discussions.

Footnotes

i We follow here the convention of using the terms ’anode’ and ’cathode’ for the negative and positive electrodes respectively.

References

  • 1.  Marlair G, Dupont L, Demissy M: Approche de la maîtrise des risques spécifiques de la filière véhicules électriques. Technical Report DRA-10-111085-11390D, INERIS, 2011. Reference Source
  • 2.  Kabza A, Fleischhammer N, Brandt K, et al.: Studie zur Bewertung der Sicherheit von Lithium-Ionen-Batterien über den gesamten Lebenszyklus. Technical report, ZSW Ulm, 2017. Reference Source
  • 3.  IEEE: Guide for the ventilation and thermal management of batteries for stationary applications. IEEE Standard 1635, 2022.
  • 4.  VDE: Hochtemperatur-Sekundärbatterien — Teil 1: Allgemeine Anforderungen. DIN EN IEC 62984-1, 2020. Reference Source
  • 5.  Leonardi SG, Samperi M, Frusteri L, et al.: A review of sodium-metal chloride batteries: materials and cell design. Batteries. 2023; 9(11): 524. Publisher Full Text
  • 6.  Benato R, Sessa SD, Crugnola G, et al.: Sodium-nickel chloride (Na-NiCl2) battery safety tests for stationary electrochemical energy storage. In: 2016 AEIT Int Annu Conf AEIT. Capri, Italy, 2016; 1–5. Publisher Full Text
  • 7.  Sudworth JL, Tilley AR, editors: The Sodium Sulfur Battery. Chapman and Hall, London, 1985. Reference Source
  • 8.  Trickett D: Current status of health and safety issues of sodium/metal chloride (Zebra) batteries. Technical Report NREL/TP-460-25553, National Renewable Energy Laboratory, Golden, Colorado, 1998. Reference Source
  • 9.  Armand M, Ortiz-Vitoriano N, Olarte J, et al.: Salt batteries: opportunities and applications of storage systems based on sodium nickel chloride batteries. European Union, 2023. Reference Source
  • 10.  Benato R, Cosciani N, Crugnola G, et al.: Sodium nickel chloride battery technology for large-scale stationary storage in the high voltage network. J Power Sources. 2015; 293: 127–136. Publisher Full Text
  • 11.  Lu X, Lemmon JP, Sprenkle V, et al.: Sodium-beta Alumina batteries: status and challenges. J Miner Met Mater Soc. 2010; 62(9): 31–36. Publisher Full Text
  • 12.  Dustmann CH: Advances in ZEBRA batteries. J Power Sources. 2004; 127(1–2): 85–92. Publisher Full Text
  • 13.  Chatwin T: Abuse testing of Sodium Nickel Chloride batteries. In: Intelec 2013; 35th International Telecommunications Energy Conference, SMART POWER AND EFFICIENCY. Hamburg, Germany, 2013; 318–323. Reference Source
  • 14.  Sudworth JL: The sodium/sulphur battery. J Power Sources. 1984; 11(1–2): 143–154. Publisher Full Text
  • 15.  Ohi JM: Environmental, health, and safety issues of sodium-sulfur batteries for electric and hybrid vehicles. Technical Report NREL/TP-262-4678, National Renewable Energy Laboratory, Golden, Colorado, 1992. Reference Source
  • 16.  Kim H, Boysen DA, Newhouse JM, et al.: Liquid metal batteries: past, present, and future. Chem Rev. 2013; 113(3): 2075–2099. PubMed Abstract | Publisher Full Text
  • 17.  Stefani F, Weier T, Gundrum T, et al.: How to circumvent the size limitation of liquid metal batteries due to the Tayler instability. Energy Convers Manag. 2011; 52(8–9): 2982–2986. Publisher Full Text
  • 18.  Kelley DH, Weier T: Fluid mechanics of liquid metal batteries. Appl Mech Rev. 2018; 70(2): 020801. Publisher Full Text
  • 19.  Chum HL, Osteryoung RA: Review of thermally regenerative electrochemical cells. Number SERI/TR-332-416. Solar Energy Research Institute, 1981. Reference Source
  • 20.  Bradwell DJ: Liquid metal batteries: ambipolar electrolysis and alkaline earth electroalloying cells. PhD thesis, Massachusetts Institute of Technology, 2011. Reference Source
  • 21.  Agruss B, Karas HR, Decker VL: Design and development of a liquid metal fuel cell. Technical Report ASD-TDR-62-1045, General Motors Corporation, 1962. Reference Source
  • 22.  Agruss B, Karas HR: First quarterly technical progress report on design and development of a liquid metal cell for the period 1 January 1962 – 31 March 1962. Technical Report AD 274 197, Armed Service Technical Information Agency, 1962.
  • 23.  Kim J: Cell design/fabrication and optimization of cell components for rechargeable all-liquid metal batteries. Master thesis, Ulsan National Institute of Science and Technology, 2017. Reference Source
  • 24.  Cairns EJ, Gay EC, Kolba VM, et al.: Lithium/Selenium secondary cells for components in electric vehicular-propulsion generating systems. Technical Report Project Order No. MERDC 175-69, Argonne National Laboratory, 1970.
  • 25.  Gay EC, Arntzen JD, Cairns EJ, et al.: Lithium/chalcogen secondary cells for components in electric vehicular-propulsion generating systems. Technical Report ANL-7863, Argonne National Laboratory, 1972.
  • 26.  Xu J, Kjos SO, Osen KS, et al.: Na-Zn liquid metal battery. J Power Sources. 2016; 332: 274–280. Publisher Full Text
  • 27.  Xu J, Martinez AM, Osen KS, et al.: Electrode behaviors of Na-Zn liquid metal battery. J Electrochem Soc. 2017; 164(12): A2335–A2340. Publisher Full Text
  • 28.  Sarma M, Lee J, Nash W, et al.: Reusable cell design for high-temperature (600 °C) liquid metal battery cycling. J Electrochem Soc. 2024; 171(4): 040531. Publisher Full Text
  • 29.  Underwriters Laboratories: Standard for safety. Energy Storage Systems and Equipment. UL 9540, 2023.
  • 30.  VDE: Hochtemperatur-Sekundärbatterien - Teil 2: Sicherheitsanforderungen und Prüfungen. DIN EN IEC 62984-2, 2021. Reference Source
  • 31.  Underwriters Laboratories: Standard for safety. Batteries for use in stationary and motive auxiliary power applications. UL 1973: 2022. Reference Source
  • 32.  Underwriters Laboratories: Test method for evaluating thermal runaway fire propagation in battery energy storage systems. UL 9540A: 2019. Reference Source
  • 33.  Ara Ake: Stationary battery energy storage systems analysis: a focus on intraday shifting. Technical report. Ara Ake, 8 Young Street, New Plymouth 4310, 2023. Reference Source
  • 34.  Safety of machinery — general principles for design — risk assessment and risk reduction. ISO 12100, 2010. Reference Source
  • 35.  Sicherheit von Maschinen - Risikobeurteilung - Teil 2: Praktischer Leitfaden und Verfahrensbeispiele. DIN ISO/TR 14121, 2013. Reference Source
  • 36.  Hamer WJ, Malmberg MS, Rubin B: Theoretical electromotive forces for cells containing a single solid or molten chloride electrolyte. J Electrochem Soc. 1956; 103(1): 8–16. Publisher Full Text
  • 37.  Temkin M: Mixtures of fused salts as ionic solutions. Acta Physicochim. URSS, 1945; 20(4): 411–420.
  • 38.  Fellner P: Comments on some models of molten salt mixtures. Chem Pap. 1983; 37: 609–615. Reference Source
  • 39.  Stephan P, Kabelac S, Kind M, editors, et al.: VDI-Wärmeatlas. Springer Reference Technik. Springer, Berlin, Heidelberg, 2019. Publisher Full Text
  • 40.  Lide DR, editor: CRC handbook of chemistry and physics. CRC Press, Boca Raton, 2005. Reference Source
  • 41.  Roine A: HSC chemistry. Metso, 2023. Reference Source
  • 42.  Auerkari P: Mechanical and physical properties of engineering alumina ceramics. Technical report 1792. Technical Research Centre of Finland (VTT), Espoo, 1996. Reference Source
  • 43.  Ginnings DC, Furukawa GT: Heat capacity standards for the range 14 to 1200 °K. J Am Chem Soc. 1953; 75(3): 522–527. Publisher Full Text
  • 44.  Kennedy MW, Zhang K, Fritzsch R, et al.: Characterization of ceramic foam filters used for liquid metal filtration. Metall Mater Trans B. 2013; 44(3): 671–690. Publisher Full Text
  • 45.  Iida T, Guthrie RIL: The thermophysical properties of metallic liquids. Oxford University Press, United Kingdom, 2015. Reference Source
  • 46.  Smithells CJ, Gale WF, Totemeier TC: Smithells metals reference book. Elsevier Butterworth-Heinemann, Amsterdam, 8th edition, 2004. Reference Source
  • 47.  Janz GJ, Tomkins RPT, Allen CB, et al.: Molten salts: Volume 4, part 2, chlorides and mixtures—electrical conductance, density, viscosity, and surface tension data. J Phys Chem Ref Data. 1975; 4: 871–1178. Publisher Full Text
  • 48.  Special Metals: The NILO® and NILOMAG® Nickel-Iron alloys. Reference Source
  • 49.  Bale CW, Bélisle E, Chartrand P, et al.: FactSage thermochemical software and databases, 2010–2016. Calphad. 2016; 54: 35–53. Publisher Full Text
  • 50.  DGUV: GESTIS substance database: information system on hazardous substances of the German social accident insurance. 2023. Reference Source
  • 51.  Hommel G: Merkblätter 1–414. Springer, Berlin, Heidelberg, 1993. Reference Source
  • 52.  National Research Council: Prudent practices in the laboratory: handling and management of chemical hazards. National Academies Press, Washington, D.C., 2011. Reference Source
  • 53.  Ladge C, Beauchamp F, Bonhomme T: French sodium school – sodium technology and sodium loop operation. 2018.
  • 54.  Guidez J: Phénix: the experience feedback. EDP Sciences, Les Ulis, 2013. Reference Source
  • 55.  Mundy CJ, Hutter J, Parrinello M: Microsolvation and chemical reactivity of sodium and water clusters. J Am Chem Soc. 2000; 122(19): 4837–4838. Publisher Full Text
  • 56.  Schröder V: Explosionsgrenzen von Wasserstoff und Wasserstoff/Methangemischen. Technical Report 253. Bundesanstalt für Materialforschung und -prüfung, Berlin, 2002.
  • 57.  Ogden JM: Prodspects for building a hydrogen energy infrastructure. Annu Rev Energy Environ. 1999; 24(1): 227–279. Publisher Full Text
  • 58.  Ladwig TH: Industrial fire prevention and protection. Van Nostrand Reinhold, New York, 1991. Reference Source
  • 59.  Kirk-Othmer: editor. Kirk-Othmer encyclopedia of chemical technology. Wiley, 2001.
  • 60.  ECHA: Opinion proposing harmonised classification and labelling at EU level of lithium carbonate [1] lithium chloride [2] lithium hydroxide [3]. Technical Report CLH-O-0000007034-82-01/F. European Chemicals Agency, 2021. Reference Source
  • 61.  United Nations: Globally Harmonized System of Classification and Labelling of Chemicals (GHS). United Nations Publication. United Nations, New York Geneva, 2021. Reference Source
  • 62.  Vale A, Bradberry S, Proudfoot A: Clinical toxicology of insecticides. In: Tim Marrs, editor. Mammalian Toxicology of Insecticides. The Royal Society of Chemistry, 2012; 312–347. Publisher Full Text
  • 63.  Bumbrah GS, Krishan K, Kanchan T, et al.: Phosphide poisoning: a review of literature. Forensic Sci Int. 2012; 214(1–3): 1–6. PubMed Abstract | Publisher Full Text
  • 64.  AGS: Verzeichnis krebserzeugender, erbgutverändernder oder fortpflanzungsgefährdender Stoffe. TRGS 905, 2005. Reference Source
  • 65.  IEEE: IEEE recommended practice for stationary battery electrolyte spill containment and management. IEEE, 2018; 1578–2018. Publisher Full Text
  • 66.  ISO: Ergonomie der thermischen Umgebung - Bewertungsverfahren für menschliche Reaktionen bei Kontakt mit Oberflächen - Teil 1: Heiße Oberflächen. 2008. DIN EN ISO 13732-1.
  • 67.  Zieger P, Väisänen O, Corbin JC, et al.: Revising the hygroscopicity of inorganic sea salt particles. Nat Commun. 2017; 8(1): 15883. PubMed Abstract | Publisher Full Text | Free Full Text
  • 68.  Wernecke R, Wernecke J, editors: Industrial Moisture and Humidity Measurement. Wiley-VCH, Weinheim, Germany, 2014.
  • 69.  Inman D, Lovering DG, editors: Ionic Liquids. Springer US, Boston, MA, 1981. Publisher Full Text
  • 70.  Janz GJ: Molten Salts Handbook. Academic Press, New York, London, 1967. Publisher Full Text
  • 71.  Williams DF: Assessment of Candidate Molten Salt Coolants for the NGNP/NHI Heat-Transfer Loop. Technical Report ORNL/TM-2006/69, Oak Ridge National Laboratory, 2006. Reference Source
  • 72.  Gardner HJ, Brown CT, Janz GJ: The preparation of dry alkali chlorides for solutes and solvents in conductance studies. J Phys Chem. 1956; 60(10): 1458–1460. Publisher Full Text
  • 73.  Ropp RC: The Alkaline Earths as Metals. In: Encyclopedia of the Alkaline Earth Compounds. Elsevier, 2013; 1–23. Publisher Full Text
  • 74.  Holleman AF, Wiberg N: Lehrbuch der anorganischen Chemie. Walter de Gruyter, Berlin, New York, 2007. Publisher Full Text
  • 75.  Patnaik P: Handbook of Inorganic Chemicals. McGraw-Hill, New York, 2003. Reference Source
  • 76.  Mellor JW: Cu, Ag, Au, Ca, Sr, Ba. Number III in A Comprehensive Treatise on Inorganic and Theoretical Chemistry. Longmans, Green and Co. Ltd., 1922.
  • 77.  Fenstad J, Fray DJ: The binary diagram water+barium chloride. C R Chim. 2006; 9(10): 1235–1242. Publisher Full Text
  • 78.  Benrath A, Lechner K: Das reziproke Salzpaar CdCl2+BaBr2=CdBr2+BaCl2. Z für anorg allg Chem. 1940; 244(4): 359–376. Publisher Full Text
  • 79.  Assarsson G: Equilibria in the ternary system MgCl2-BaCl2-H2O between 18 and 100°. J Phys Chem. 1956; 60: 1436–1439.
  • 80.  Duval C: Inorganic Thermogravimetric Analysis. Elsevier, Amsterdam, London, New York, 1963.
  • 81.  Lumpkin JA, Perlmutter D: Thermal and water vapor effects on the rate of the dehydration reactions of barium chloride. Thermochim Acta. 1995; 249: 335–349. Publisher Full Text
  • 82.  Ekberg C, Brown PL: Hydrolysis of metal ions. WILEY-VCH, Weinheim, Germany, 2016. Publisher Full Text
  • 83.  Bellobono IR, Marcandalli B, Selli E, et al.: Thermodynamic analysis of the reaction of barium chloride with water vapour from 1173 to 1473K. Mater Chem Phys. 1984; 10(2): 163–174. Publisher Full Text
  • 84.  Baes CF, Mesmer RE: The hydrolysis of cations. Wiley-Interscience, New York, Sydney, London, Toronto, 1976. Reference Source
  • 85.  Neumann B, Kröger C, Jüttner H: Die Systeme Erdalkalichlorid-Erdalkalioxyd und die Zersetzung der Erdalkalichloride durch Wasserdampf. Zeitschr Elektrochem. 1935; 41(10): 725–736. Publisher Full Text
  • 86.  Pátek J, Klomfar J, Součková M: Solid-Liquid equilibrium in the system of CaCl2-H2O with special regard to the transition points. J Chem Eng Data. 2008; 53(10): 2260–2271. Publisher Full Text
  • 87.  Schiffries CM: Liquid-absent aqueous fluid inclusions and phase equilibria in the system CaCl2-NaCl-H2O. Geochim Cosmochim Acta. 1990; 54(3): 611–619. Publisher Full Text
  • 88.  Li D, Zeng D, Yin X, et al.: Phase diagrams and thermochemical modeling of salt lake brine systems. II. NaCl+H2O, KCl+H2O, MgCl2+H2O and CaCl2+H2O systems. Calphad. 2016; 53: 78–89. Publisher Full Text
  • 89.  Ally MR: Predicting phase diagram of the CaCl2 ·H2O binary system from the BET adsorption isotherm. Fluid Ph Equilib. 2008; 268(1–2): 45–50. Publisher Full Text
  • 90.  Qiao C, Suraneni P, Weiss J: Phase diagram and volume change of the Ca(OH)2-CaCl2-H2O system for varying Ca(OH)2/CaCl2 molar ratios. J Mater Civ Eng. 2018; 30(2): 04017281. Publisher Full Text
  • 91.  Zeng D, Xu W, Voigt W, et al.: Thermodynamic study of the system (LiCl+CaCl2+H2O). J Chem Thermodyn. 2008; 40(7): 1157–1165. Publisher Full Text
  • 92.  Pitzer KS, Shi Y: Thermodynamics of calcium chloride in highly concentrated aqueous solution and in hydrated crystals. J Solut Chem. 1993; 22(2): 99–105. Publisher Full Text
  • 93.  Pitzer KS, Oakes CS: Thermodynamics of calcium chloride in concentrated aqueous solutions and in crystals. J Chem Eng Data. 1994; 39(3): 553–559. Publisher Full Text
  • 94.  Molenda M, Bouché M, Linder M, et al.: Thermochemical energy storage for low temperature applications: materials and first studies in a gas-solid reactor. In: International Conference on Energy Storage. 2012; 1–10. Reference Source
  • 95.  Mellor JW: Ra and Ac Families, Be, Mg, Zn Cd, Hg. Number IV in a comprehensive treatise on inorganic and theoretical chemistry. Longmans, Green and Co. Ltd., 1929. Reference Source
  • 96.  Smith DM, Neu MP, Garcia E, et al.: Hydration of plutonium oxide and process salts, NaCl, KCl, CaCl2, MgCl2: effect of calcination on residual water and rehydration. Waste Manag. 2000; 20: 479–490. Publisher Full Text
  • 97.  Meisingset KK, Gronvold F: Thermodynamic properties and phase transitions of salt hydrates between 270 and 400 K IV. CaCl2 ·6H2O, CaCI2 ·4H2O, CaCI2 ·2H2O, and FeCl3 ·6H2O. J Chem Thermodyn. 1986; 18: 159–173. Publisher Full Text
  • 98.  Wiley VCH, editor: Ullmann’s encyclopedia of industrial chemistry. Wiley, 2007.
  • 99.  Molenda M, Stengler J, Linder M, et al.: Reversible hydration behavior of CaCl2 at high H2O partial pressures for thermochemical energy storage. Thermochim Acta. 2013; 560: 76–81. Publisher Full Text
  • 100.  Bischoff JL, Rosenbauer RJ, Fournier RO: The generation of HCI in the system CaCl2-H2O: vapor-liquid relations from 380-500◦C. Geochim Cosmochim Acta. 1996; 60(1): 7–16. Publisher Full Text
  • 101.  Gonzalez M, Faulkner E, Zhang C, et al.: Electrochemical methods for analysis of hydroxide and oxide impurities in Li, Mg/Na, and Ca based molten chloride salts. ECS Trans. 2020; 98(10): 161–169. Publisher Full Text
  • 102.  Tomkute V, Solheim A, Olsen E: CO2 capture by CaO in molten CaF2-CaCl2 : optimization of the process and cyclability of CO2 capture. Energy Fuels. 2014; 28(8): 5345–5353. Publisher Full Text
  • 103.  Kondo H, Asaki Z, Kondo Y: Hydrolysis of fused calcium chloride at high temperature. Metall Trans B. 1978; 9(3): 477–483. Publisher Full Text
  • 104.  Olsen E, Hansen M, Nygård HS: Hydrolysis of molten CaCl2-CaF2 with additions of CaO. AIMS Energy. 2017; 5(6): 873–886. Publisher Full Text
  • 105.  Vainio E, DeMartini N, Hupa L, et al.: Hygroscopic properties of calcium chloride and its role on cold-end corrosion in biomass combustion. Energy Fuels. 2019; 33(11): 11913–11922. Publisher Full Text
  • 106.  Natsui S, Shibuya R, Suzuki RO, et al.: Quantification of the impact of residual H2O on cathodic behavior in molten CaCl2 electrolysis. J Sustain Metall. 2022; 8(1): 532–540. Publisher Full Text
  • 107.  Fife KW, Bowersox DF, Christensen DC, et al.: The preparation of fused chloride salts for use in pyro-chemical plutonium recovery operations at los alamos. Technical Report LA-10681, Los Alamos National Laboratory, 1986. Reference Source
  • 108.  Huguet L, Barge-Zwick V, Bars ML: Dynamics of a reactive spherical particle falling in a linearly stratified fluid. Phys Rev Fluids. 2020; 5(11): 114803. Publisher Full Text
  • 109.  Wang X, Hu Q, Kim GP, et al.: Experimental study of the hygroscopy of single and different mixtures of MgCl2, KCl, NaCl, ZnC2 for application as heat transfer fluid in CSP. In: Proc ASME. Pittsburgh, 2018; 1–10. Publisher Full Text
  • 110.  Smirnov MV, Korzun IV, Oleynikova VA: Hydrolysis of molten alkali chlorides, bromides and iodides. Electrochim Acta. 1988; 33(6): 781–788. Publisher Full Text
  • 111.  Johnson CR: Hydrolysis of alkali chlorides. J Phys Chem. 1935; 39(6): 791–796. Publisher Full Text
  • 112.  Briner E, Roth P: Recherches sur l’hydrolyse par la vapeur d’eau de chlorures alcalins seuls ou additionnés de divers adjuvants. Helv Chim Acta. 1948; 31(5): 1352–1360. PubMed Abstract | Publisher Full Text
  • 113.  Sohr J, Schmidt H, Voigt W: Higher hydrates of lithium chloride, lithium bromide and lithium iodide. Acta Crystallogr C Struct Chem. 2018; 74(Pt 2): 194–202. PubMed Abstract | Publisher Full Text
  • 114.  Monnin C, Dubois M, Papaiconomou N, et al.: Thermodynamics of the LiCl + H2O System. J Chem Eng Data. 2002; 47(6): 1331–1336. Publisher Full Text
  • 115.  Li D, Zeng D, Han H, et al.: Phase diagrams and thermochemical modeling of salt lake brine systems. I. LiCl+H2O system. Calphad. 2015; 51: 1–12. Publisher Full Text
  • 116.  Pátek J, Klomfar J: Solid-liquid phase equilibrium in the systems of LiBr-H2O and LiCl-H2O. Fluid Phase Equilib. 2006; 250(1–2): 138–149. Publisher Full Text
  • 117.  Kamali AR, Fray DJ, Schwandt C: Thermokinetic characteristics of lithium chloride. J Therm Anal Calorim. 2011; 104(2): 619–626. Publisher Full Text
  • 118.  Masset PJ: Thermogravimetric study of the dehydration reaction of LiCl·H2O. J Therm Anal Calorim. 2009; 96(2): 439–441. Publisher Full Text
  • 119.  Burkhard WJ, Corbett JD: The solubility of water in molten mixtures of LiCl and KCl. J Am Chem Soc. 1957; 79(24): 6361–6363. Publisher Full Text
  • 120.  Laitinen HA, Ferguson WS, Osteryoung RA: Preparation of pure fused lithium chloride-potassium chloride eutectic solvent. J Electrochem Soc. 1957; 104(8): 516. Publisher Full Text
  • 121.  Swain L, Ghosh S, Pakhui G, et al.: Redox behavior of Moisture in LiCl-KCl eutectic melts: a cyclic voltammetry study. Nucl Technol. 2021; 207(1): 119–146. Publisher Full Text
  • 122.  Anderko A, Pitzer KS: Phase equilibria and volumetric properties of the systems KCl-H2O and NaCl-KCl-H2O above 573K: equation of state representation. Geochim Cosmochim Acta. 1993; 57(20): 4885–4897. Publisher Full Text
  • 123.  Niazi S, Nygård HS, Reis B, et al.: Consistent thermodynamic modeling of H2O-HCl-KOH-KCl between 200 K and 1,000 K. Chem Eng Sci. 2022; 264: 118209. Publisher Full Text
  • 124.  Steiger M: Thermodynamic properties of SrCl2(aq) from 252 K to 524 K and phase equilibria in the SrCl2-H2O system: implications for thermochemical heat storage. J Chem Thermodyn. 2018; 120: 106–115. Publisher Full Text
  • 125.  Clark RJ, Farid M: Hydration reaction kinetics of SrCl2 and SrCl2-cement composite material for thermochemical energy storage. Sol Energy Mater Sol Cells. 2021; 231: 111311. Publisher Full Text
  • 126.  Blijlevens MAR, Mazur N, Kooijman W, et al.: A study of the hydration and dehydration transitions of SrCl2 hydrates for use in heat storage. Sol Energy Mater Sol Cells. 2022; 242: 111770. Publisher Full Text
  • 127.  Gavini SN, Vyas SN: Solvents effects on solubility and dehydration of strontium chloride. J Chem Eng Data. 1979; 24(4): 258–261. Publisher Full Text
  • 128.  Tanaka H, Shimada S, Negita H: The kinetic study of thermal dehydration stages of SrCl2 · 2H2O and its deuterium analog. Int J Chem Kinet. 1985; 17(2): 149–156. Publisher Full Text
  • 129.  Follner H, Brehler B: Die Kristallstruktur des ZnCl2·4/3H2O. Acta Cryst. 1970; B26: 1679–1682. Publisher Full Text
  • 130.  Pillai SB, Wilcox RJ, Hillis BG, et al.: Understanding the water-in-salt to salt-in-water characteristics across the Zinc Chloride: water phase diagram. J Phys Chem B. 2022; 126(11): 2265–2278. PubMed Abstract | Publisher Full Text
  • 131.  Hennings E, Schmidt H, Voigt W: Crystal structures of ZnCl2·2.5H2 ZnCl2·3H2 and ZnCl2·4.5H2O. Acta Crystallogr Sect E Struct Rep Online. 2014; 70(Pt 12): 515–518. PubMed Abstract | Publisher Full Text | Free Full Text
  • 132.  Wilcox RJ, Losey BP, Folmer JCW, et al.: Crystalline and liquid structure of Zinc Chloride trihydrate: a unique Ionic liquid. Inorg Chem. 2015; 54(3): 1109–1119. PubMed Abstract | Publisher Full Text
  • 133.  Kirilenko IA: Glass formation in the ZnCl2-H2O system. Russ J Inorg Chem. 2013; 58(10): 1183–1186. Publisher Full Text
  • 134.  Jones F, Tran H, Lindberg D, et al.: Thermal stability of zinc compounds. Energy Fuels. 2013; 27(10): 5663–5669. Publisher Full Text
  • 135.  Threlfall R: The electrolysis of molten Zinc Chloride. J Soc Chem Ind. 1929; 48(30). Publisher Full Text
  • 136.  Niazi S: Experimental and theoretical evaluation of thermodynamic properties of low melting chlorides suitable for liquefaction of biomass. PhD thesis, Norwegian University of Life Sciences, 2022. Reference Source
  • 137.  Watson RF, Perry GS: Solubility of ZnO and hydrolysis of ZnCl2 in KCI melts. J Chem Soc Faraday Trans. 1991; 87(18): 2955–2960. Publisher Full Text
  • 138.  Niazi S, Olsen E, Nygård HS: Hydrolysis of eutectic compositions in the ZnCl2: KCl:NaCl ternary system and effect of adding ZnO. J Mol Liq. 2020; 317: 114069. Publisher Full Text
  • 139.  Hamilton HGC: Hydrolytic and associated reactions in molten zinc chloride-sodium chloride. PhD thesis, Imperial College of Science, Technology and Medicine, London, 1989.
  • 140.  Bloom H, Welch BJ: The vapor pressure of cadmium and zinc chlorides. J Phys Chem. 1958; 62(12): 1594–1595. Publisher Full Text
  • 141.  Keneshea FJ, Cubicciotti D: Vapor pressures of zinc chloride and zinc bromide and their gaseous dimerization. J Chem Phys. 1964; 40(1): 191–199. Publisher Full Text
  • 142.  Richtlinie 2014/68/EU des Europäischen Parlaments und des Rates vom 15. Mai 2014 zur Harmonisierung der Rechtsvorschriften der Mitgliedstaaten über die Bereitstellung von Druckgeräten auf dem Markt. Directive 2014/68/EU. 2014. Reference Source
  • 143.  Emons HH, Bräutigam G, Thomas R: Dampfdruckmessungen an binären geschmolzenen Mischungen aus Erdalkalimetall- und Alkalimetallchloriden. Chem Zvesti. 1976; 30(6): 773–782.
  • 144.  International Atomic Energy Agency: Thermophysical properties of materials for nuclear engineering: a tutorial and collection of data. International Atomic Energy Agency, Vienna, 2008. Reference Source
  • 145.  Boerboom AJH, Reyn HW, Kistemaker J: Heat of sublimation and vapour pressure of strontium. Physica. 1964; 30(1): 254–257. Publisher Full Text
  • 146.  Emons HH, Kiessling D, Horlbeck W: Dampfdruckmessungen und massenspektrometrische Untersuchungen der Gasphase über Erdalkalimetallhalogeniden. Z Für Anorg Allg Chem. 1982; 488(1): 219–222. Publisher Full Text
  • 147.  Janz GJ, Allen CB, Bansal NP, et al.: Physical properties data compilations relevant to energy storage. II. molten salts: Data on Single and Multi-Component Salt Systems. U. S. Department of Commerce, Troy, New York, 1979. Reference Source
  • 148.  Hoffman JW, Lauder I: Basic Zinc Chlorides. Aust J Chem. 1968; 21(6): 1439–1443. Publisher Full Text
  • 149.  Reid CE: Chemical thermodynamics. McGraw-Hill, New York, 1990. Reference Source
  • 150.  Emons HH, Voigt W: Zur Chemie geschmolzener Salze. Akademie-Verlag, 1981. Publisher Full Text
  • 151.  Manga VR, Bringuier S, Paul J, et al.: Molecular dynamics simulations and thermodynamic modeling of NaCl–KCl–ZnCl2 ternary system. Calphad. 2014; 46: 176–183. Publisher Full Text
  • 152.  Romero-Serrano A, Hernandez-Ramirez A, Cruz-Ramirez A, et al.: Optimization and calculation of the MCl–ZnCl2 (M=Li, Na, K) phase diagrams. Thermochim Acta. 2010; 510(1–2): 88–92. Publisher Full Text
  • 153.  Iida T, Guthrie RIL: The physical properties of liquid metals. Oxford Science Publications. Clarendon Press, Oxford, 1988. Reference Source
  • 154.  Redkin AA, Zaykov YP: Relation between the thermal expansion coefficient and the heat capacity in halide melts. Russ Metall Met. 2017; 2017(2): 75–78. Publisher Full Text
  • 155.  Lide DR, editor: CRC handbook of chemistry and physics: a ready-reference book of chemical and physical data. CRC Press, Boca Raton, Fla., 1995. Reference Source
  • 156.  Meisel P: Werkstoffliche und technologische Entwicklungen für keramische Wärmerohre zur Hochtemperaturanwendung. PhD thesis, Technische Universität Dresden, 2016. Reference Source
  • 157.  Pelton AD: The Ag-Na (Silver-Sodium) system. Bull Alloy Phase Diagr. 1986; 7(2): 133–136. Publisher Full Text
  • 158.  Ma S, Xing J, Fu H, et al.: Interfacial morphology and corrosion resistance of Fe–B cast steel containing chromium and nickel in liquid zinc. Corros Sci. 2011; 53(9): 2826–2834. Publisher Full Text
  • 159.  Xu J, Bright MA, Liu X, et al.: Liquid metal corrosion of 316l stainless steel, 410 stainless steel, and 1015 carbon steel in a molten zinc bath. Metall Mater Trans A. 2007; 38(11): 2727–2736. Publisher Full Text
  • 160.  Han K, Ohnuma I, Okuda K, et al.: Experimental determination of phase diagram in the Zn-Fe binary system. J Alloys Compd. 2018; 737: 490–504. Publisher Full Text
  • 161.  Cammerer WF: Wärme- und Kälteschutz. Springer, Berlin, Heidelberg, 5th edition, 1995. Publisher Full Text
  • 162.  Arbeitsgemeinschaft Industriebau e.V: Mineralwolle als Dämmstoff für betriebstechnische Anlagen. AGI Q 132, 2006.
  • 163.  Arbeitsgemeinschaft Industriebau e.V: Calcium-Magnesium-Silikatfaster (CMS-Faser) als Dämmstoff für betriebstechnische Anlagen. AGI Q 140, 2002. Reference Source
  • 164.  Friatec: Electrical feedthroughs and insulating tubes: ceramic-to-metal components. Product catalogue, 2023.
  • 165.  Danzer R, Lube T, Supancic P, et al.: Fracture of ceramics. Adv Eng Mater. 2008; 10(4): 275–298. Publisher Full Text
  • 166.  Kyocera: Elektro- und beschleunigertechnik. Keramik-Metall-Verbundbauteile aus Hochleistungskeramik. Product catalogue, 2023. Reference Source
  • 167.  GSI: Internationaler Schweißfachingenieurlehrgang. Gesellschaft für Schweißtechnik International mbH, 2010.
  • 168.  Sobolev V: Database of thermophysical properties of liquid metal coolants for GEN-IV. Technical Report SCK•CEN-BLG-1069, SCK CEN, Mol, Belgium, 2011. Reference Source
  • 169.  Wittenberg LJ, DeWitt R: Volume contraction during melting; emphasis on lanthanide and actinide metals. J Chem Phys. 1972; 56(9): 4526–4533. Publisher Full Text
  • 170.  Bloom H: The chemistry of molten salts. W. A. Benjamin, Inc., New York, Amsterdam, 1967. Reference Source
  • 171.  IEC: Sicherheitsanforderungen an Sekundar-Batterien und Batterieanlagen - Teil 1: allgemeine Sicherheitsinformationen. IEC 62485-1, 2019. Reference Source
  • 172.  IEC: Sicherheitsanforderungen an Sekundar-Batterien und Batterieanlagen - Teil 2: stationäre Batterien. IEC 62485-2, 2019. Reference Source
  • 173.  Vetter KJ: Electrochemical kinetics. Elsevier Science, Burlington, 1967. Reference Source
  • 174.  Bagotsky VS: Fundamentals of electrochemistry. The Electrochemical Society Series. Wiley-Interscience, Hoboken, New Jersey, 2006. Publisher Full Text
  • 175.  Delimarskii IK, Markov BF: Electrochemistry of fused salts. The Sigma Press, Washington, D.C., 1961. Reference Source
  • 176.  Dinh LN, McLean II M, Schildbach MA, et al.: The nature and effects of the thermal stability of lithium hydroxide. J Nucl Mater. 2003; 317(2–3): 175–188. Publisher Full Text
  • 177.  Ambri: Technology. Ambri, 2019. Reference Source
  • 178.  Thompson G, Bradwell DJ, Pujari V, et al.: Ceramic materials and seals for high temperature reactive material devices. World patent WO2016141354A2, 2022. Reference Source
  • 179.  Informationsstelle Edelstahl Rostfrei: Nichtrostende und hitzebeständige Stähle bei hohen Temperaturen. Technical Report Merkblatt 987. Informationsstelle Edelstrahl Rostfrei, Düsseldorf, 2023. Reference Source
  • 180.  Wegener E: Festigkeitsberechnung verfahrenstechnischer Apparate. Wiley, 2002. Reference Source
  • 181.  Wegst C, Wegst M: Stahlschlüssel. Verlag Stahlschlüssel Wegst GmbH, Marbach, 20th edition, 2004.
  • 182.  Hylok: Hy-Lok Klemmringverschraubungen. Katalog H-200TF-D, Hy-Lok D Vertriebs GmbH, 2023. Reference Source
  • 183.  Sensorshop24: Drucktransmitter G1/4" oder G1/2" für Über- und Unterdruck mit Normstecker (0-10V/4-20mA). Product datasheet, 2023. Reference Source
  • 184.  Muhs D, Wittel H, Jannasch D, et al.: Roloff/Matek Maschinenelemente: Normung, Berechnung, Gestaltung. Springer, Wiesbaden, 2005. Reference Source
  • 185.  VDI: Systematic calculation of highly stressed bolted joints - joints with one cylindrical bolt. VDI 2230, 2015. Reference Source
  • 186.  Valbruna: Valbruna AN 5 / Alloy 286 / 1.4980. Materials datasheet, 2023. Reference Source
  • 187.  Baggio A, D’Isanto F, Valenza F, et al.: The joining of alumina to hastelloy by a TiZrCuNi filler metal: wettability and interfacial reactivity. Materials. 2023; 16(5): 1976. Publisher Full Text
  • 188.  Stephens JJ, Burchett SN, Hosking FM: High temperature creep properties of eutectic and near eutectic silver- copper alloys: application to metal/ceramic joining. Technical Report SAND-91-0006C; CONF-911003-10: DE91017987, Sandia National Laboratories, Albuquerque, United States, 1991. Reference Source
  • 189.  Weber N, Duczek C, Marquez GM, et al.: Data publication: risk assessment for Na-Zn liquid metal batteries. May 2024. Reference Source